Fwd: Welding Consumable - SA 479 410SS (Control valve seal retainer)

50 views
Skip to first unread message

Sanjay Viswanathan

unread,
Apr 20, 2023, 4:47:45 AM4/20/23
to material...@googlegroups.com



I have to repair / re thread a threaded portion of a 3" control valve seal retainer (Material is SA 479 410SS).

What will be the suitable consumable for this?

Service: Boiler feed water pump outlet.
Size : 3" 1500#
Body: A216 WCB

Thanks & Best Regards

Sanjay

Vishwas Keskar Welding Manager WELDING

unread,
Apr 20, 2023, 11:20:18 PM4/20/23
to Materials & Welding
PL. SEND DRAWING/WELDING CONFIGURATION

Mehrab Chakoshkar

unread,
Apr 20, 2023, 11:20:23 PM4/20/23
to Materials & Welding
You can use E410 and sometimes E309, But for your case, my best suggestion is ERNiCrMo-3 because your service operation is associated with corrosion and erosion and further there is carbon steel material there that will be joined to SS.
ER CrNiMo-3
GTAW if possible
Preheat for thk>1" about 100 C
if you wanna healing the surface use AC plus 50-50%

james gerald

unread,
Apr 21, 2023, 3:36:41 AM4/21/23
to material...@googlegroups.com
I suppose It is a seal weld in Valve Trim part. Try ER 309L or ER NiCr3 for TIG welding.  Since this is a martensitic stainless steel the base material SS 410 has to be preheated to 200DegC while welding. 3inch control valve amd I suppose warming using TIG torch before welding will suffice.

Thanks & Regards

J.Gerald Jayakumar



--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.