PWHT on Stainless steel to Carbon Steel Weld

119 views
Skip to first unread message

Shahil Saini

unread,
Jun 7, 2023, 6:58:13 AM6/7/23
to material...@googlegroups.com
Hello everyone,
Good Evening,
hope all are doing well,

As my subject indicates PWHT in SS to CS Weld joint, my question is what are the after effects if pwht performed in SS to CS joint??

In Addition, how to mitigate the after effects which occurred after pwht?

BM: SS 316L to SA516 Gr.70 

Kannayeram Gnanapandithan

unread,
Jun 8, 2023, 2:27:00 AM6/8/23
to material...@googlegroups.com
CARBIDE FORMATION, tO AVOID, BUTTER CARBON STEEL WITH NICKEL BASE ELECTRODE LIKE NICRMO3 OR NICR3, CARRY OUT PWHT, AFTER THAT WELD WITH SS 316 WITH ABOVE SAID ROD

THANKS & BEST REGARDS,
KG.PANDITHAN, BE, IWE,  CSWIP 3.1,
ISO 9712 Level 2 in VT,
ASNT-Level II in PT,MT,RT & UT,
LA ISO 9001-2015,
International Welding Engineer. 
CONSULTANT-WELDING & QUALITY
Mobile no: +919940739349


--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CALfBO_8bejT55kYnUkJTc5p_DQD7ZRUkb1x%3DRA4u_oNgZTtG0A%40mail.gmail.com.

Parminder Singh

unread,
Jun 8, 2023, 2:43:09 AM6/8/23
to material...@googlegroups.com
Buttering of 516 Gr 70 with 309LMo, Then perform PWHT 
then Weld 316L to Buttered CS. 

On Wed, Jun 7, 2023 at 4:28 PM Shahil Saini <sainis...@gmail.com> wrote:
--

Kannayeram Gnanapandithan

unread,
Jun 8, 2023, 8:05:10 AM6/8/23
to materials-welding
at cs pwht temp, carbide formation??

Vishwas Keskar Welding Manager WELDING

unread,
Jun 13, 2023, 12:23:41 AM6/13/23
to Materials & Welding
Dear Shahil 
Pl furnish below information :
Why PWHT is required  ?
What is type of joint ?
What is PWHT Holding temperature and Holding time ?
Which type of filler metal that is planed to be used ?
What is service of the equipment ?Corrosive  or Elevated Temp.(If yes what is temp)

Thanks and regards

Vishwas - IWE International Welding Engineer