Welding rod for EN 1.7221 material

133 views
Skip to first unread message

ambrish dubey

unread,
Feb 22, 2015, 1:04:31 AM2/22/15
to material...@googlegroups.com
Dear All,
can anybody help me to decide which filler material is suitable for welding EN1.7221 material

Thanks,
Ambrish

Manivannan Hemu

unread,
Feb 23, 2015, 9:38:47 AM2/23/15
to material...@googlegroups.com
Dear Ambrish,

For SMAW You can select E 8016 C1.

Regards,
MANIVANNAN



--
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To post to this group, send email to material...@googlegroups.com.
Visit this group at http://groups.google.com/group/materials-welding.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/0a135847-c3f6-4949-8e56-fae1cb3673c9%40googlegroups.com.
For more options, visit https://groups.google.com/d/optout.

ambrish dubey

unread,
Feb 23, 2015, 11:38:11 PM2/23/15
to material...@googlegroups.com
Dear manivannam,

thanks for advice , but the rod is nickel based , and the e1.7221 chemistry there is no nickel , its chromium based ,

Thanks,
Ambrish

Manivannan Hemu

unread,
Mar 4, 2015, 12:02:21 PM3/4/15
to material...@googlegroups.com
Hi,
You can refer to standard SEW 685, which provides recommend welding electrode as:
-ESY 42 37 2 Ni 6 (contain 2% Ni)
-ESY 55 76 2 Ni Mo B (contain 2% Ni)
-ESY 50 55 1 Ni Mo B
These designation and typical chemical you can get from DIN 8529 part 1.