PWHT holding time range for Pqr acc.to EN15614-1

591 views
Skip to first unread message

nirvana kz

unread,
Oct 5, 2014, 11:04:40 PM10/5/14
to material...@googlegroups.com
Hello friends,

I have a question about welding procedure qualification with post weld heat treatment which will be prepared as per EN 15614-1.

Material 13CrMo4-5 group number 5.1 as per ISO 15608. Material thickness 25m and diameter 273mm.

As per EN 13480-4 it requires Pwht holding time (2xt) = 50 minutes.

As per EN 15614-1, t=25mm thickness, qualification thickness range is 12.5<t<50mm.

 

If we do pqr with holding time 50 minutes,

1.       Does it qualify 50mm thickness with Pwht (as per EN 13480-4 t=50mm requires 100minutes holding time)

2.       What will be holding time for t=12.5mm material at reality (it will be same as pqr which we hold 50minutes, if so there is conflict with EN 13480-4 because as per this standard t=12.5mm require 25 minutes holding)

3.       For to qualify pqr in case weld repair after pwht, what shall be my holding time?

Pwht subject is not clear for me on procedure qualification. Hence there is several pqr I need to prepare and most of them with Pwht. I hesitate if the pqr which I prepare will not qualify repair weld after PWHT.

I need your help about issue.

Thanks in advance.

 

Karthik

unread,
Oct 6, 2014, 4:21:10 AM10/6/14
to material...@googlegroups.com
Hi,
Please find below my suggestions as marked in Red.

If we do pqr with holding time 50 minutes,
1.       Does it qualify 50mm thickness with Pwht (as per EN 13480-4 t=50mm requires 100minutes holding time) - EN13480-4 specifis the minimum holding time and EN15614-1 restricts holding temperature and the holding temperature shall not deviate 20 degree celsius (plus or minus) to the qualified procedure.According to EN15614-1,Section 8.4.12; heating rate,cooling rate and holding time shall be related to the product. So in your case you go for 100 minutes holding time with holding temperaure of 670 to 720 degree celsius.
2.       What will be holding time for t=12.5mm material at reality (it will be same as pqr which we hold 50minutes, if so there is conflict with EN 13480-4 because as per this standard t=12.5mm require 25 minutes holding) - No conflict., EN13480 specifies the minimum holding time.
3.       For to qualify pqr in case weld repair after pwht, what shall be my holding time?
Pwht subject is not clear for me on procedure qualification. Hence there is several pqr I need to prepare and most of them with Pwht. I hesitate if the pqr which I prepare will not qualify repair weld after PWHT.
I need your help about issue.
Thanks in advance. - According to EN13480-4,section 9.14.1; If there is any repair done after PWHT., follow as per table 9.14.1(I Suggest you qualify your PQR with 2 cycles)
 
Hope it clear
 
Thanks & Regards,

(Karthik)

Karthikeyan.S
QA/QC Manager
German-Thai Boiler Engineering Cooperation Limited.
Rayong Factory ;
379 Moo.6 Soi 8, Tambol Pananikom,
Nikompattana, Rayong 21180 THAILAND
Tel : +66 38 897 035-9 Ext. 137
Hand Phone: 0066 892512282




--
To post to this group, send email to material...@googlegroups.com
To unsubscribe from this group, send email to materials-weld...@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
For more options, visit https://groups.google.com/d/optout.


nirvana kz

unread,
Oct 6, 2014, 11:55:51 PM10/6/14
to material...@googlegroups.com
Hi Mr Karthik,

Thank you for your reply. It is really very helpful.

I want to ask one more question for clarify.

If we do pqr (t=25mm, will qualify thickness 12.5<t<50mm) with holding time 200 minutes for to qualify 50mm thickness 2 times (considering the repair), the qualified thickness 12.5mm will be 8 times qualified. it means we can do repair welding several times (as long as company procedure permit), and there will not be any problem to prepare Wps for thickness  t=12.5mm from that Pqr with holding time 25minutes , am i right?

Shortly, as long as holding temperature are within limits (+/- 20 degree Celsius as per EN15614-1 8.4.12), for holding time i will consider qualified the tickest tickness (x2 cycle - in case of repair)  from EN13480-4 table 9.14.1-1 and i can prepare Wps for qualified the thinnest material. 

Best regards.


Date: Sun, 5 Oct 2014 21:28:37 -0700
From: material...@googlegroups.com
Subject: Re: [MW:22040] PWHT holding time range for Pqr acc.to EN15614-1
To: material...@googlegroups.com

Karthik

unread,
Oct 7, 2014, 4:07:02 AM10/7/14
to material...@googlegroups.com
Yes, up to your actual production weld requiremrnts
 
Thanks & Regards,

(Karthik)

Karthikeyan.S
QA/QC Manager
German-Thai Boiler Engineering Cooperation Limited.
Rayong Factory ;
379 Moo.6 Soi 8, Tambol Pananikom,
Nikompattana, Rayong 21180 THAILAND
Tel : +66 38 897 035-9 Ext. 137
Hand Phone: 0066 892512282


Reply all
Reply to author
Forward
0 new messages