WPS and PQR According to ASME Sec.IX and Sec.VIII- Boiler and Pressure Vessel Code

609 views
Skip to first unread message

K K

unread,
Oct 24, 2020, 12:59:35 AM10/24/20
to Materials & Welding
Dear Experts,

Please refer below WPS and PQR details.

PQR Details - Base Metal - ASTM A106 Gr.B  To ASTM A106 Gr.B. ( P No - 1 Gr.No - 1 To  P No - 1 Gr.No - 1 ).
Process - GTAW  + SMAW ( GTAW - 4.8 mm + SMAW - 13.46 mm)
Thickness of the Coupon -18.26 mm, Dia - 6"
With PWHT - 638°C ,time 72 min.
No Impact tested.
DESIGN TEMP. / MDMT (°C) -290 / 5 .

WPS Details - Base Metal - ASTM A106 / A516 Gr.B / Gr.70  To  ASTM A106 / A516 Gr.B / Gr.70 . ( P No - 1 Gr.No - 1/2 To  P No - 1 Gr.No - 1/2 ).
Process - GTAW  + SMAW ( GTAW - 9.6 mm + SMAW - 15.4 mm).
SFA No- GTAW - 5.18 and for SMAW - 5.1.
AWS No - GTAW - ER70S-3 and SMAW - E7018-1H4R.
Pre heat - less than 12.7 mm -10°C and less than 25 mm 75°C.
Inter pass Temp. -315°C.
PWHT - 620°C, Holding time 1 hr thk +1 hour min.

According to above details help me to review, as per ASME Section VIII for Boiler and Pressure Vessel Code.
And I need your suggestion what are the essentials requirements according ASME  Sec.VIII. And what are the important things i have to check.
Please suggested me with clause reference.

Please send me your valuable suggestions, it's Supports me lot.

Thanks and Regards
Kiran




 

Jamie R

unread,
Oct 24, 2020, 8:58:23 AM10/24/20
to Materials & Welding
 your query is kind of broad. You should only involve the essential and non essential variables for each weld process used, stated in ASME Section IX. To involve ASME Sect. VIII without knowing what it is you are trying to incorporate, one would only be guessing. In short, there is no "essential requirements" when creating a weld procedure specification that you will find in a code of construction. Follow ASME IX and refer to the code of construction as needed.

Hany Nabil

unread,
Oct 24, 2020, 8:58:24 AM10/24/20
to material...@googlegroups.com
Dear Sir,

For welding qualification ( WPS )
You have to follow ASME- IX , not ASME VIII

Thanks & Regards,

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/c3e78183-f533-400b-bfe1-ba8e24f94c6an%40googlegroups.com.
--


 Best Regards,

 Eng. Hany Nabil
 Senior Welding Engineer
 Petrofac
 Engineering and Production Service
 Egypt Mobile: 002-01225622022




This message, including any attachments, may contain confidential and privileged information for the sole use of the intended recipient(s). Review, use, distribution or disclosure by others is strictly prohibited. If you are not the intended recipient, or authorised to receive information on behalf of the recipient, please contact the sender by reply email, and delete all copies of this message. While we have taken reasonable precautions to ensure that this message and any attachments are free from viruses, we cannot guarantee that they are virus free and accept no liability for any damage caused by this message or any attachments. Messages sent or received through our networks may be monitored to ensure compliance with the law, regulation and/or our policies.

José Juan Jiménez Alejandro

unread,
Oct 24, 2020, 11:56:31 AM10/24/20
to material...@googlegroups.com
For your Welding procedures (WPS and the respective PQR) you must use ASME BPVC Section IX, but if your construction code is ASME BPVC Section VIII Div. 1 you must see in this Code the preheating suggested in the Non-mandatory Appendix R, and you should see what is related to PWHT in this Code, which has some tables and graphs for this topic, in other words there is data that you have to take from your Building Code; Get advice from your Authorized ASME Inspector if you have a contract with an Authorized Inspection Agency.
Greetings!.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.


--

Ing. José Juan Jiménez Alejandro

Independent Consultant in Parts

and Pressure Equipment

SUMMIT MÉXICO - TPI

https://www.linkedin.com/in/summit-m%C3%A9xico-tpi-760047137/

Móvil +52 1 812 352 4606

Skype: jjjimeneza





Vishwas Keskar

unread,
Oct 27, 2020, 7:45:35 AM10/27/20
to material...@googlegroups.com
WPS is ok  as per ASME SEC IX to be used for ASME  SEC VIII DIV 1 vessel with no impact testing required for this vessel.
By why PWHT is specified ?

Thickness seems to be very less 

Pl. check with design data of Engineering drawing 

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.

George Dilintas

unread,
Nov 3, 2020, 5:25:30 AM11/3/20
to material...@googlegroups.com
impact test requirements  when the Code of Construction is VIII-1 
You start from UG-20 Design Temperature to check for exceptions and then you go to UCS-65 & 66 & 67 in case of CArbon or Low Alloy Steel, not to forget UG-84 for test plates requirments

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/c3e78183-f533-400b-bfe1-ba8e24f94c6an%40googlegroups.com.


--
Dr. Georgios Dilintas,
Dipl. Ing. In Aeronautic and Space Engineering
Ph.D in Mechanics of Solids - Computational Mechanics
A.I.S, A.N.I, IRCA Lead Auditor
Welding, Stress Analysis, Corrosion, QA/QC, Failure Analysis, Risk Analysis

Bien_ND

unread,
Nov 6, 2020, 7:20:10 AM11/6/20
to Materials & Welding
I think it may ok. Next to follow variable in QW-250.
Same filling data and format at here.