Tube to Tube sheet welds_Minimum Leak Path Measurement _REg.,

2,868 views
Skip to first unread message

kcrtechnical

unread,
Aug 18, 2011, 10:57:04 PM8/18/11
to material...@googlegroups.com
Dear all,
 
Can you share with me about minium leak path measurement and its acceptance crietaria as per ASME Section I.
 
Best regards
K C R

meisam shokri arfaei

unread,
Aug 19, 2011, 5:11:15 AM8/19/11
to material...@googlegroups.com
Dear Sir (from KCR),
Whould you please clarify which on of below is your requirement?
1 - you like to measure the like path when you do macro test?
2 - you like to know designing parameters for leak path?
 
Regards

--
To post to this group, send email to material...@googlegroups.com
To unsubscribe from this group, send email to materials-weld...@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.



--
M.Shokri Arfaei
International Welding Engineer
RT, UT ASNT Level III
ERI-Metallurgy Lab. Manager
Tel: +98 21 66283693
Fax: +98 21 66283693
Mob.: +98 912 139 4023
Web: www.metallurgylab.com

Pieper QSI

unread,
Aug 19, 2011, 7:54:59 AM8/19/11
to material...@googlegroups.com

Dear KCR,

 

Leak Path is defined as the shortest way in any direction on a macro/micro specimen between the inside of the tube and the gap between tube and tube-plate, see example below. The maximum value will be the thickness of the tubes wall thickness, but because of improper welding this can become less when weld thickness is not sufficient. As far as I know the minimum acceptable value should be specified by your customer and is not mentioned anywhere in ASME section I.

 

 

 

Through Weld A (green) the path is longer than the thickness of the tube wall t and therefore Leak Path will be t.

The thickness of Weld B (red) is smaller as the tube wall t, here the shortest dimension measured through the weld will be the Leak Path.

 

 

 

 

 

 

Hope this makes things clear for you.

 

 

Met vriendelijke groeten / Best Regards

 

Herman Pieper

 

Pieper Quality Support & Inspection