[MW:5239] Use of MIG filler wire as a TIG welding filler wire

23 views
Skip to first unread message

hitesh patel

unread,
May 25, 2010, 4:08:18 AM5/25/10
to material...@googlegroups.com
Dear friends,


i am going to use below ER316LMn filler wire for SS316L. (working condition 4.5K ( -269 'C ) temp.)

ER316LMn filler wire available for TIG & MIG welding. i want to use 1.2 mm dia. filler wire for TIG welding but 1.2 mm dia. not available for TIG welding. 

as 1.2 mm dia. filler available in MIG welding. filler wire mfg. given property for ER316LMn listed below for GTAW & GMAW.

if i want to use MIG filler wire for TIG welding , can I get TIG welding property listed below.

Please give your valuable suggestions.  


Mechanical properties, typical, all weld metal for filler wire ER316LMn

                            Process              Shielding              Condition             0.2% Proof strength              Tensile strength                Elongation               Impact ISO-V(J)
                                                         gas                                                (N/mm2)                                (N/mm2)                          (%)                        -196°C

Typical values          GTAW                  I1                       AW                        430                                        650                               35                              75
                              GMAW                 M12                    AW                        400                                        600                               30                             50



Thanks & Regards,

Hitesh

--
To post to this group, send email to material...@googlegroups.com
To unsubscribe from this group, send email to materials-weld...@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

Roy LIU刘艺

unread,
May 25, 2010, 6:17:07 AM5/25/10
to material...@googlegroups.com
Hi, Hitesh,
From my own experience, I think it is available to use MIG wire for TIG process.
The reasons of different property are the shielding gas and welding procedure.

I1=100% Argon
M12=5↓%CO2 + 95↑%Argon
Generally, the property under pure Argon condition is higher than the condition with Oxidizing gas.
 
and the layer of TIG welding is a little more than MIG welding.
Heat Input of TIG welding is lower too.
 
So do not hesitate to use this wire as TIG wire as long as you can control the welding procedure.
 

 

Best regards

 

Roy LIU

 

Böhler Welding Group - China

you may contact me via roy...@bw-group.com.cn
 

Date: Tue, 25 May 2010 13:38:18 +0530
Subject: [MW:5239] Use of MIG filler wire as a TIG welding filler wire
From: hpa...@ipr.res.in
To: material...@googlegroups.com

使用新一代 Windows Live Messenger 轻松交流和共享! 立刻下载!

N VENKATESWARA PRASAD

unread,
May 25, 2010, 9:14:06 AM5/25/10
to material...@googlegroups.com
Dear Mr. Hitesh,
 
The TIG and MIG filler wires are  manufactured as per same SFA specification only difference is that you get in spool form for MIG welding and cut length form for TIG welding.  You can use the MIG wire for TIG welding with out any deviation in properties.
 
Regards
 
N.V. PRASAD
WELDING ENGINEER
VELOSI CERTIFICATION, QATAR