Filler material Selection

199 views
Skip to first unread message

Navanith

unread,
Dec 23, 2019, 12:25:39 AM12/23/19
to Materials & Welding
Dear Experts,

Require guidance on filler material selection as per ASME BPVC.
For example:I received this query from a client
Base metal is ASTM A106 Gr.B and they want to weld using E316L electrodes.
Is it possible to use E316L electrodes to weld directly?

Regards,
Navanith

anand gupta

unread,
Dec 23, 2019, 6:05:05 AM12/23/19
to material...@googlegroups.com
Dear 
If base metal is SA 106 GR B then why u r going for SS316L. 

Simple go for  ER70S2/E7018

REGARDS 
A P GUPTA 
BARODA 
--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/37bac14e-c9a8-4d35-af83-c5e116da3bc8%40googlegroups.com.

Kannayeram Gnanapandithan

unread,
Dec 23, 2019, 6:05:12 AM12/23/19
to materials-welding
Use 309

--

Kannayeram Gnanapandithan

unread,
Dec 23, 2019, 10:08:36 PM12/23/19
to materials-welding
Pl refer B31.1 , chapter V, 128 and give your opinion , when joining Austenitic material with other like C's, weldmetal structure should have Austenitic structure. Thanks

HENNING John

unread,
Dec 23, 2019, 10:08:37 PM12/23/19
to material...@googlegroups.com

Possible, yes, but not for Section I if water wetted service.

 

Practical, no, absolutely not.  I have a really difficult time trying to come with any reason to do this and a host of possible issues if done.

 

Enjoy - John

--

https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/37bac14e-c9a8-4d35-af83-c5e116da3bc8%40googlegroups.com.

DISCLAIMER This e-mail and any attachments thereto may contain information which is confidential and/or protected by intellectual property rights and are intended for the sole use of the recipient(s)named above. Any use of the information contained herein (including, but not limited to, total or partial reproduction, communication or distribution in any form) by persons other than the designated recipient(s) is prohibited. If you have received this e-mail in error, please notify the sender either by telephone or by e-mail and delete the material from any computer.
General Data Protection Regulation (GDPR)
We respect and protect your privacy to provide you with our services. Please read https://www.hamon.com/customer-data-protection-notice (Customer) and https://www.hamon.com/seller-data-protection-notice (Supplier) how we process your personal data.

Thank you for your cooperation.
______________________________________________________________________

Navanith

unread,
Dec 26, 2019, 3:02:52 AM12/26/19
to material...@googlegroups.com
Received clarification from the client about using E316L to weld Carbon steel.
Their welders are qualified to weld steel (P1 to P15) with filler material (F1 to F4).
They want these welder to be qualified for F No. 5 but do not have austenitic steel base metal in stock. Only Carbon steel is available in stock.
Therefore, they have requested a PQR to weld Carbon steel base metal P No 1 with E316L and ER 316L (F5 and F6).
In case the coupon meets ASME Section IX Nondestructive and destructive testing requirements, they will prepare a WPS which shall be used only to qualify welders for F number.

On another note, I hope to receive guidance on selection of filler materials in general. 
What are the parameters to be considered to select filler materials for any base metal and whether it is addressed by general standards in the industry.

Thanks and best regards,
Navanith




Jason

unread,
Dec 27, 2019, 1:15:44 AM12/27/19
to Materials & Welding
ASTM A106 Gr.B  is Carbon steel,E316L electrodes are used for stainless steel

在 2019年12月23日星期一 UTC+3上午8:25:39,Navanith写道:

Kannayeram Gnanapandithan

unread,
Dec 28, 2019, 3:49:02 AM12/28/19
to materials-welding
While welding CS with 316, ( chemistry 19Cr+12Ni), there is loss in Cr and Ni more 316 when compare with 309( 24Cr+13). For maintaining austenetic structure in ASS( as per code B31.1, which is attached) minimum requirement of Ni is 8, which may not be achievable with 316. So, it is better to use 309 instead of 316


THANKS & BEST REGARDS,
KG.PANDITHAN, BE, IWE,  CSWIP 3.1,
ISO 9712 Level 2 in VT,
ASNT-Level II in PT,MT,RT & UT,
LA ISO 9001-2015,
International Welding Engineer. 
CONSULTANT-WELDING & QUALITY
Mobile no: +919940739349


--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
ASME B31.1.pdf
Reply all
Reply to author
Forward
0 new messages