ASME SEC IX...PWHT?

1,036 views
Skip to first unread message

Nandesh Kumar

unread,
Jan 26, 2010, 4:33:23 AM1/26/10
to material...@googlegroups.com
Dear All,
 
For our LNG piping project, as per ASME SEC IX for a pipe 16 inch OD and Thk 21.44 mm PWHT is manadtory? We are welding root and hot pass TIG and others SMAW.
Material is ASTM A333 .
 
Thaks in advance
Nandesh Kumar A


Your Mail works best with the New Yahoo Optimized IE8. Get it NOW!.

Chandra, Vasanthan (Lagos)

unread,
Jan 26, 2010, 5:18:57 AM1/26/10
to material...@googlegroups.com

Nandesh,

 

PWHT requirement is to be cross referred in line with Construction/Design code. In your mail, the applicable design code is missing. However, assuming the design code as B31.3 (2008) for piping, PWHT is mandatory for a thickness >20mm.

 

Regards,
Vasanth


--
To post to this group, send email to material...@googlegroups.com
To unsubscribe from this group, send email to materials-weld...@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.


*** WORLEYPARSONS GROUP NOTICE *** "This email is confidential. If you are not the intended recipient, you must not disclose or use the information contained in it. If you have received this email in error, please notify us immediately by return email and delete the email and any attachments. Any personal views or opinions expressed by the writer may not necessarily reflect the views or opinions of any company in the WorleyParsons Group of Companies."

Antonio Ruscitto

unread,
Jan 26, 2010, 5:30:22 AM1/26/10
to material...@googlegroups.com
ASME IX is not a code that can determine the PWHT, you must use a code of construction like being ASME B31.3 or ASME VIII. Soon you must determine N° P and the group that ASTM A333 corresponds, since there are different considerations for what has been said
Ruscitto

>>> Nandesh Kumar <nandes...@rocketmail.com> 26/01/2010 06:33 am >>>
--
To post to this group, send email to material...@googlegroups.com
To unsubscribe from this group, send email to materials-weld...@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

*********************************************************************

¡IMPORTANTE!

Para evitar accidentes por inhalación de monóxido de carbono:

- Mantenga los ambientes ventilados en forma permanente.

- Revise que la llama sea color azul y uniforme.

- Instale y haga revisar periódicamente sus artefactos sólo a través de gasistas matriculados.

Recuerde que los artefactos a gas pueden emitir Monóxido de Carbono: un gas altamente tóxico e imperceptible.

Más consejos en http://www.metrogas.com.ar

*********************************************************************

Este mensaje es privado y confidencial y va dirigido sólo al destinatario indicado. Si lo ha recibido por error, por favor avísenos inmediatamente vía e-mail a error...@metrogas.com.ar y tenga la amabilidad de eliminarlo de su sistema. La utilización o divulgación de su contenido puede importar la comisión de un delito. No copie, reproduzca o divulgue -en forma parcial o total- su contenido. Cualquier opinión contenida, es exclusiva de su autor y no representa la opinión de MetroGAS S.A. - Muchas gracias.

This message is private and confidential and it is only intended for the addressee named above. If you have received this message and it is not addressed to you, please advise us immediately at error...@metrogas.com.ar and kindly remove it from your system. The use or disclosure of its contents may be regarded as an offense. Do not copy, reproduce or disclose them, either partially or fully. Opinions are the exclusive responsibility of the author and do not represent the opinion of MetroGAS S.A. - Thank you.

:: http://www.metrogas.com.ar

 

A D

unread,
Jan 26, 2010, 8:22:18 AM1/26/10
to material...@googlegroups.com
Hi Nandesh,
                    For PWHT requirement detail is not given in ASME Sec IX, it is required based on construction code and Client specification.
 
As per ASME B31.3 , generally PWHT  required  for A333 Gr.6 is above 20 mm thk, but based on service fluid it will be higher requirement than code.
 
In my previous shell project some services requirement is 100%.
 
Louis
Singapore
 
 
--- On Tue, 26/1/10, Nandesh Kumar <nandes...@rocketmail.com> wrote:

From: Nandesh Kumar <nandes...@rocketmail.com>
Subject: [MW:4150] ASME SEC IX...PWHT?
--
To post to this group, send email to material...@googlegroups.com
To unsubscribe from this group, send email to materials-weld...@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.


The INTERNET now has a personality. YOURS! See your Yahoo! Homepage.

pgoswami

unread,
Jan 26, 2010, 10:48:51 PM1/26/10
to material...@googlegroups.com

Nandesh,

 

Looking at your query, if the material of construction is P No/S No-1 then PWHT is mandatory over ¾” or 20 mm pipe wall thickness. This is the PWHT criteria as per B-31.3 -2008 code.

 

If the design code is not B-31.3 then PWHT requirements of the applicable design code will follow. Do you have impact requirements for LNG piping if so @ what temperature?.

 

If you could provide those details e.g. materials grade, SA 333 Gr1 or 6 , design code, design temperature more comprehensive answers could be provided.

 

Thanks

 

Pradip Goswami, P.Eng

88,Garth Trails Crescent

Hamilton,Ontario, L9B2X1,Canada

Email-p...@sympatico.ca

Email-p...@quickclic.net

 


Nandesh Kumar

unread,
Jan 28, 2010, 12:08:05 AM1/28/10
to material...@googlegroups.com
Dear Mr. Pradeep,
 
Yes you are right. Please throw some more light on this issue
 
Material : ASTM A333 Gr. 6
Design code : ASTM B31.3
Service : LNG line
Impact requirement : yes @ -21° C
 
Thanks for the suggestions.
Nandesh

--- On Wed, 27/1/10, pgoswami <pgos...@quickclic.net> wrote:

rajagopal kannan

unread,
Jan 28, 2010, 2:52:13 AM1/28/10
to material...@googlegroups.com
Dear Nandesh,
 
As Per Table - A1, A333gr.6 is exempted from impact testing until -45 Deg.
How there could be an impact requirement @ -21 Deg.C.
 
Can you please clarify.
Thanks and Best regards,
K.Rajagopal

mohammed faisal ahmed shareef

unread,
May 27, 2016, 2:49:07 AM5/27/16
to Materials & Welding
Hi All ;
As per the latest Edition of ASME B31.3 2014 all materials for PNo 1 are exempt from PWHT .I don't have a current copy but this is the link

George Dilintas

unread,
May 27, 2016, 10:55:19 PM5/27/16
to Meghanadh K
Yes subject to the conditions stated on 331.1.3.
My personal advise: follow the requirements of 31.1 (power piping) on this matter


The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To post to this group, send email to material...@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/7c53cbab-7caf-4c08-a2cc-2ddccafecc6a%40googlegroups.com.
For more options, visit https://groups.google.com/d/optout.



--
Dr. Georgios Dilintas,
Dipl. Ing. In Aeronautic and Space Engineering
Ph.D in Mechanics of Solids - Computational Mechanics
A.I.S, A.N.I, IRCA Lead Auditor
Welding, Stress Analysis, Corrosion, QA/QC, Failure Analysis, Risk Analysis