Re: [MW:23846] Re: ASTM A36 plates for pressure vessels

982 views
Skip to first unread message

Raghuram Bathula

unread,
Nov 3, 2015, 1:21:34 AM11/3/15
to Materials-Welding
In addition Code Case 2811 provides guidelines for use of  SA/EN 10025-2 Steel Grades S235J2, S275J2, and S355J2   in fabrication of pressure vessels

https://www.linkedin.com/grp/post/122787-6061068041251278851?trk=groups-post-b-title

On 3 November 2015 at 10:12, Abhay Pethe <agp...@gmail.com> wrote:
SA-36 is permitted for use in construction of pressure vessels according to UCS-6 of the ASME BPVC. Practically nobody uses the same remains the fact.

No comments regarding the equivalency or use of A36 in place of A234.


Best Regards,
Abhay Pethe

On 30 October 2015 at 06:54, Plate Steel <er...@ysteelplate.com> wrote:
Dear Syed,

Firstly A36 is just one common carbon structural steel,this steel plate can make common tanks,but not pressure vessels.Because,As a professional steel supplier,we knew when rolling A36,no need to do Ultrasonic test,but for pressure vessel used steel,they have to be done Ultrasonic test.

Second,your said A234 is one pressure vessel steel,actually another pressure vessel steel ASTM A285GrC is similar to A234.

It would be dangerous if using A36 to replace of A234,Freind.

Eric 

在 2011年1月24日星期一 UTC+8下午9:36:28,Moin - QC写道:

Dear members,

Can a plate to ASTM A36 can be used to manufacture TEEs to A234 WPB, is there any restriction in BPV or B31.3 on the use of A36 plate for manufacturing A234 Tees.

One of client says A36 is for general purpose and cannot be used for making a pressure containing component to be used in oil and gas production . Is it correct, if yes why? And if not can you please provide me a technical justification, I could not find anything B31.3.

Thanks & Regards
Syed Moin                               


JIGNESH RANA

unread,
Nov 3, 2015, 10:06:58 PM11/3/15
to material...@googlegroups.com
dear Syed, 

strictly,code, there is no limitation on raw material for the products to be certified as per A 234, except it shall meets with chemical requirements of particular grade. 
If specific requirements based on service (like NACE), then restricted chemistry applies. 

regards, 

jignesh rana 

--
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To post to this group, send email to material...@googlegroups.com.
Visit this group at http://groups.google.com/group/materials-welding.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CADxVubm111HFHayhmwPOOyE7K34hOjbhuG8gizMFi1yj%2BX4CmQ%40mail.gmail.com.
For more options, visit https://groups.google.com/d/optout.

pgoswami

unread,
Nov 3, 2015, 11:51:57 PM11/3/15
to material...@googlegroups.com

Hello Syed,

 

You should use A-36 steel for making fittings. Please see the materials requirements for A 234 fitting vs. the Scope for A-36 material. The text narrated below  is self explanatory. Any killed grade of C-Mn steel would be a good substitute for A-36 subject to the design requirements.

 

Thanks.

 

 

Pradip Goswami, P.Eng,IWE

Welding & Metallurgical Engineering Specialist

Hamilton, Ontario, Canada

pgos...@quickclic.net

pradip....@gmail.com

ca.linkedin.com/pub/pradip-goswami/5/985/299

 

SA-234/SA-234M

 

Materials 5.1 The material for fittings shall consist of killed steel, forgings, bars, plates, seamless or fusion-welded tubular products with filler metal added and shall conform to the chemical requirements of Table 1. Unless otherwise specified for carbon steel plates, the steel may be made to either coarse grain or fine grain practice

 

SA-36/SA-36M:-

1. Scope

1.1 This specification covers carbon steel shapes, plates, and bars of structural quality for use in riveted, bolted, or welded construction of bridges and buildings, and for general structural purposes


Ritesh Rajput

unread,
Nov 4, 2015, 12:28:34 AM11/4/15
to material...@googlegroups.com
Dear syed .

I  hope you are from gerab ,Dubai ,

As per the A 36 plate standard , This plate can not use  in Pipe construction or in the Fitting construction .

because it is structural steel material grade.

where our application of ASTM A 234 WPB fitting is in process piping .

Both are Different ,

We faced same Problem in one of our reputed customer , but finally on the basis of the Chemical composition and mechanical test perform on laboratory and satisfied customer and End users .

Submit one stated letter from the manufacturer to Client about the suitability of  raw material .

Thank you very much 

Best of regards

Ritesh Rajput 



pgoswami

unread,
Nov 4, 2015, 9:42:23 PM11/4/15
to material...@googlegroups.com

To All,

 

A small correction in my response as below.

 

Thanks.

 

 

Pradip Goswami, P.Eng,IWE

Welding & Metallurgical Engineering Specialist

Hamilton, Ontario, Canada

pgos...@quickclic.net

pradip....@gmail.com

ca.linkedin.com/pub/pradip-goswami/5/985/299


From: material...@googlegroups.com [mailto:material...@googlegroups.com] On Behalf Of pgoswami
Sent: Tuesday, November 03, 2015 11:52 PM
To: material...@googlegroups.com
Subject: RE: [MW:23850] Re: ASTM A36 plates for pressure vessels

 

Hello Syed,

 

You should  NOT use A-36 steel for making fittings. Please see the materials requirements for A 234 fitting vs. the Scope for A-36 material. The text narrated below  is self explanatory. Any killed grade of C-Mn steel would be a good substitute for A-36 subject to the design requirements.