Pitting Corrosion Test ASTM G48 Method A for SS 316L Materials

660 views
Skip to first unread message

stephen raj

unread,
Nov 28, 2023, 12:18:54 PM11/28/23
to Materials & Welding
Dear Sir,
For SS316L material, we performed the Pitting Corrosion Test ASTM G48 Method A in accordance with the client's specifications and acceptance criteria, and we followed ISO 17781 standards in accordance with the client's standard reference.


We failed the test, and the weight reduction ranged from 50 to 500 g. It should be 1g according to the standard.


Can somebody advise or explain why this test failed?

BR

Stephenraj.s

Ashish Chacko

unread,
Nov 29, 2023, 4:05:56 AM11/29/23
to Materials & Welding
Can u let us know what was the type of material pipe or plate or whether it was welded?

james gerald

unread,
Nov 29, 2023, 4:05:56 AM11/29/23
to material...@googlegroups.com
What is the Testing temperature, normally 316L is suitable at 10degC.

If the root is oxidised due to inadequate purging, there may be a possibility

Thanks & Regards

J.Gerald Jayakumar




--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/4a981284-81b7-410e-9472-6219dfe085a9n%40googlegroups.com.

Stephenraj

unread,
Nov 29, 2023, 8:49:50 AM11/29/23
to material...@googlegroups.com
It is raw material Seam less 316L pipe 

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.

james gerald

unread,
Nov 29, 2023, 8:49:52 AM11/29/23
to material...@googlegroups.com
Raw material Plate or pipe  will be tested in the Mill before procuring. My assumption is to be PQR test coupon

Thanks & Regards

J.Gerald Jayakumar


--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To view this discussion on the web visit

P Goswami

unread,
Nov 29, 2023, 9:59:49 AM11/29/23
to material...@googlegroups.com

ASTM G48A test is a very aggressive test. It’s like a Go-No Go test, with respect to Pitting. Usually, this test is not called for in SS 316L. For all Offshore Oil & Gas application usually  this test is called for Duplex & Super Duplex Grades , 6Mo & Alloy 625.

 

The temperature and the duration of the test are important. See the temperature of the test to be adopted vs the duration in the ASTM G48A specification.

 

Typically, if one tries to exercise the common conditions for testing on DSS/ SDSS on SS 316L then Failures are inevitable. It’s good to know why this test is called for on SS 316L and what’s the intended service? Please ask your client.  If the intended service is offshore , then the testing temperature & duration should be the least applicable as per ASTM G48A.

 

Generally speaking, ASTM, A 262, Practice E or C are the recommended corrosion tests for SS 316L.

 

Refer the attached blogs for some additional guidance.

 

Thanks.

 

 

Pradip Goswami.P.Eng, IWE.

Welding & Metallurgical Engineering Specialist

Linkedin: https://www.linkedin.com/in/pradip-goswami-2999855/

Email:pgos...@rogers.com,pradip....@gmail.com

Cell/Whasapp:1-905-9793232

G 48 - 11 (2015).pdf
ASTM G48A Test, Blogs.pdf

james gerald

unread,
Dec 2, 2023, 1:21:43 PM12/2/23
to material...@googlegroups.com
Just to share. Below snap shot.

Inline image


Thanks & Regards

J.Gerald Jayakumar


On Thursday, 30 November, 2023 at 02:18:30 pm IST, james gerald <gerr...@yahoo.com> wrote:


This seems surprising Client specification calling for G48A Terst for 316L. What is the service and what is the level of Chloride ppm in service. What is the PREN requirement.

Please share the Snap shot of Client spec.

james gerald

unread,
Dec 2, 2023, 1:21:43 PM12/2/23
to material...@googlegroups.com
This seems surprising Client specification calling for G48A Terst for 316L. What is the service and what is the level of Chloride ppm in service. What is the PREN requirement.

Please share the Snap shot of Client spec.

Tn Wednesday, 29 November, 2023 at 07:19:44 pm IST, Stephenraj <arokk...@gmail.com> wrote:

Prasad rao

unread,
Dec 4, 2023, 6:36:33 AM12/4/23
to material...@googlegroups.com
What is the test duration  please share failed lab report 

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.