Consumable MTC Review

200 views
Skip to first unread message

limesh M

unread,
Nov 3, 2010, 3:19:54 AM11/3/10
to Materials & Welding
Dear All,
 
Design Code- ASME B31.3
Welding Code - ASME SEC IX
Process - GTAW+SMAW
 
I have a WPS which is qualified with PWHT and impact test.Now I have to review some consumable MTC.I need advise on the following queries. 
 
1.Is it mandatory that the consumable MTC shall show the mechanical test values with PWHT for acceptance ?
 
2.Can I accept consumable MTC which is matching with corresponding SFA and material properties with out PWHT? 
 
 
Regards,
 
 
Limesh

Karthik

unread,
Nov 3, 2010, 3:27:17 AM11/3/10
to material...@googlegroups.com

Hi,

Check Sec.II Part - C for corresponding consumable specification and test requirements.If Part-C require PWHT for your consumable then the consumable manufacturer should be done and shown on the MTC.


Thanks & Regards,

(Karthik)

Karthikeyan.S
QA/QC Manager
Getabec Energy Co.,Ltd.
379,Moo6,Soi8,Nikhomphatana,
Rayong-21180,
Thailand.
Phone: 0066 38 897035-8 (Off)
Fax: 0066 38 897034
Hand Phone: 0066 892512282


--- On Wed, 11/3/10, limesh M <lime...@gmail.com> wrote:
--
To post to this group, send email to material...@googlegroups.com
To unsubscribe from this group, send email to materials-weld...@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

george....@gr.bureauveritas.com

unread,
Nov 8, 2010, 3:29:11 AM11/8/10
to material...@googlegroups.com

YOU CAN ACCEPT THE MTC IF IT DOES HAVE THE SAME F-No

Dr. G. Dilintas - Authorized Inspector Supervisor
I&F Regional Technical Manager
Bureau Veritas Piraeus - Greece
Tel: +30 210 40 63 113/4
Fax: +30 210 40 63 118
Cell: +30 69 44 64 62 04

Inactive hide details for limesh M <limesh78@gmail.com>limesh M <lime...@gmail.com>



To


cc


Subject


    [MW:8031] Consumable MTC Review


Ref

--

To post to this group, send email to material...@googlegroups.com
To unsubscribe from this group, send email to materials-weld...@googlegroups.com
For more options, visit this group's bolg at

Vikas Bhandari

unread,
Nov 9, 2010, 7:05:12 AM11/9/10
to material...@googlegroups.com
Hi Limesh

The electrode has to so through the same PWHT as specified in your procedure qualification.Regardless of what is said in Sec II part C. (because you are heat treating the weld metal also
during your procedure qualification). U need to prove that your electrode will perform in this condition.

Regards

--