How to protect Serration of Flanges during Hot dip galvanization

2,496 views
Skip to first unread message

aly mhaskar

unread,
Aug 23, 2010, 4:38:56 AM8/23/10
to material...@googlegroups.com
Dear All,
Presently we are doing hot dip galvanization of pipe spools where we have to protect the serration of flanges during galvanization.
 
Can any body suggest what can be applied on serration to protect it from adhesion of ZINC on serration.
 
Thank you in advance.
 
Mhaskar Aly
Kuwait

Chaitanya Purohit

unread,
Aug 23, 2010, 6:29:01 AM8/23/10
to material...@googlegroups.com

Molycoat

is the high temperature grease which can withstand beyond 900 deg C. Check with supplier / manufacturer to use the same for your said application.

l am not sure but I hope it will serve your purpose

Regards..

santosh bhandary

unread,
Aug 23, 2010, 7:01:40 AM8/23/10
to material...@googlegroups.com
AT WHAT TEMPERATURE HOT DIP GALVANIZATION IS DONE?

Aly

unread,
Aug 23, 2010, 2:03:42 PM8/23/10
to material...@googlegroups.com
The Galvanization temperature is 450 Deg C . 
 
 
 
-------Original Message-------
--
To post to this group, send email to material...@googlegroups.com
To unsubscribe from this group, send email to materials-weld...@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
 
FREE Animations for your email - by IncrediMail! Click Here!
panda_hello.gif
stampa_girl_line_en.gif

Richard Bonardo

unread,
Aug 25, 2010, 4:39:16 AM8/25/10
to material...@googlegroups.com
Aly :

I have done it before,and it just working fine. It is true that there are small amount of melting zinc will fill the gaps between serration but per my past experience there are still enough roughness to hold the gasket.

I did it on 2 ", 4 " and 6 " flanges for your info.

Regards
Richard Bonardo
QA/QC Engineer
PHE-ONWJ



From: Aly <mhask...@gmail.com>
To: material...@googlegroups.com
Sent: Tue, 24 August, 2010 1:03:42 AM
Subject: Re: [MW:0] How to protect Serration of Flanges during Hot dip galvanization
panda_hello.gif
stampa_girl_line_en.gif

MNS

unread,
Aug 25, 2010, 8:39:37 AM8/25/10
to Materials & Welding
Molykote 1000 of Dow Corning Product will withstand upto 650 deg C,
anyway you can apply that uniformly and do hot dipping; but ensure no
removal of the coating while dipping.

Hamid Jabbari

unread,
Feb 10, 2016, 11:00:37 PM2/10/16
to Materials & Welding
Does any one know how could i remove the hot galvanized coating from face of flange?
plz advise

Shridev Kurup

unread,
Feb 12, 2016, 12:12:25 AM2/12/16
to material...@googlegroups.com

Dear Hamid,
Galvanised flanges mostly used in utility services  not in hydrocarbon service where leak and leakage is  catastrophic.  If galvanising is applicable in to your project flanges than specific requirements of flange seration roughnes will not be there in specs and piping class. Please read the applicable piping class material requirements. Gaskets types will compensate on the galvanised face.

If required before galv.additional temporary  arrangements can be prepared with thin metal sheets but that also will not give full assurance.

But please reverify against your requirements and address this to your client or customer.

If already this product is mistakenly galvanised than machining will be only solution on loose flanges. .and very difficult on spools.
Regards

--
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To post to this group, send email to material...@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/75d1da68-c97b-4709-b526-afb7cfd25136%40googlegroups.com.
For more options, visit https://groups.google.com/d/optout.

Perumal Govindan

unread,
Mar 4, 2016, 1:57:24 AM3/4/16
to material...@googlegroups.com

Hi
I am forgetting the cheminal name, which will be applied on the serrated surface before HDG bath, once done it will be cleaned to recover the serration.

Requested to contact the HDG agencies for more details.

With kind regards
Govindan
Kuwait

Perumal Govindan

unread,
Mar 4, 2016, 2:02:47 AM3/4/16
to material...@googlegroups.com

Hi

Request Client to accept or re machine it with the manufacturer or machine shops.

No chemical is available to clean, since the serrated surfaces might have fused.

With kind regards
Govindan

On 11 Feb 2016 07:00, "Hamid Jabbari" <lif...@gmail.com> wrote:

Shashank Vagal

unread,
Mar 4, 2016, 10:58:23 PM3/4/16
to material...@googlegroups.com
Removing galvanizing:
Try using 50% dilute HCl, dip your part in it till the bubbling stops, then wash off / rub off with baking soda.
Vinegar also is useful. 
But take care not to inhale fumes.
 

BR,
Shashank C Vagal 



From: Perumal Govindan <perumal...@gmail.com>
To: material...@googlegroups.com
Sent: Friday, 4 March 2016 7:56 AM
Subject: Re: [MW:24429] Re: How to protect Serration of Flanges during Hot dip galvanization

Reply all
Reply to author
Forward
0 new messages