Dear sir,

What will be effect in Oxidation in SS 304 root weld.

please expain.

Regards

Lalit Vadadoriya
Dy.Manager(Inspection)
Engineers India Limited

Dahej Petrochemical Complex,
Dahej (Gujarat)

Vanchinath S.A.

unread,
Apr 29, 2016, 11:54:27 PM4/29/16
to material...@googlegroups.com

Corrosion resistance will be affected.

--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To post to this group, send email to material...@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAKjb_1%2B54DqiQKhH7R%2Bfws_san5BDHLasMYRMr1GcnpWZR1Ttw%40mail.gmail.com.
For more options, visit https://groups.google.com/d/optout.

Mohd Siraj

unread,
Apr 29, 2016, 11:54:30 PM4/29/16
to Materials & Welding
Oxidisation lower its corrosiin resistance capacity.And reduce service life.
Its depend on fluid service.in case of instument air effect will slow but case of DM water and corrosive fluid effect is very fast.

LALIT VADADORIYA

unread,
May 3, 2016, 9:39:28 AM5/3/16
to material...@googlegroups.com
Dear Sir,

Oxidation of the root bead and adjacent HAZ during welding of stainless steels is commonly called heat-tint. A chromium-rich scale is formed, which is typically not very protective, and the stainless steel surface becomes chromium-depleted: these effects may impair the corrosion resistance of stainless steel welds.

Tests performed in various corrosive environments have shown that susceptibility to pitting and crevice corrosion is greater when the surface is heat-tinted, and the colour of the heat-tint is an indicator of the degree of susceptibility to corrosion. For example, purple-blue oxides are generally the most susceptible to corrosion attack. The critical pitting temperature, which is an indicator of corrosion resistance in aqueous chloride media, may be reduced from 60 to 40°C for a type 316 stainless steel weld in 0.1% NaCl solution with an applied potential of +300 mV SCE. In order to restore corrosion resistance, the scale and the Cr-depleted layer must be removed by post-weld cleaning.

An efficient back purge will minimise the formation of heat-tint. The oxygen content in the back shield must be controlled prior to the start of welding and should be minimised. Most specifications require that the back purge be maintained until the root and hot pass, and sometimes the first few fill passes, are completed or until the temperature of the root region is below about 250°C. However, it may be beneficial to reduce the gas flow pressure slightly after the root pass to stop an over-pressure build up. This is particularly important where the root bead is thin and is nearly re-melted by the second bead. The use of pure argon as backing gas is recommended. Argon/nitrogen backing gases produce good results when welding highly alloyed stainless steels, such as duplex and super-austenitic stainless steels


Regards

Lalit Vadadoriya
Dy.Manager(Inspection)
Engineers India Limited

Dahej Petrochemical Complex,
Dahej (Gujarat)

On Sat, Apr 30, 2016 at 9:16 AM, Mohd Siraj <mohd...@gmail.com> wrote:
Oxidisation lower its corrosiin resistance capacity.And reduce service life.
Its depend on fluid service.in case of instument air effect will slow but case of DM water and corrosive fluid effect is very fast.
--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To post to this group, send email to material...@googlegroups.com.
Reply all
Reply to author
Forward
0 new messages