Use of PQR (Multiple process) in making WPS(single process)

2,029 views
Skip to first unread message

Biplab Pal

unread,
Jun 1, 2013, 3:25:45 AM6/1/13
to materials-welding
Dear Experts,

I have a PQR of combine of process of GTAW (3mm)+ SMAW(12mm)+ SAW.(25mm).
Can i qualify an WPS only with GTAW with max 6 mm with other condition of the GTAW process remain same.
Can i qualify another WPS only with SMAW max 24 mm with other conditions of the SMAW process remain same.
No Impact is required.
Please give me the ASME Sec-IX references.


--
Thanks & Regards
Biplab Pal
Welding Inspector
E-mail:   bipla...@gmail.com
 
Information in this email and any attachments is confidential and intended solely for the use of the individual(s) to whom it is addressed or otherwise directed. Please note that any views or opinions presented in this email are solely those of the author and do not necessarily represent those of the Company. Finally, the recipient should check this email and any attachments for the presence of viruses. Myself accepts no liability for any damage caused by any virus transmitted by this email.
 

kannayeram gnanapandithan

unread,
Jun 3, 2013, 12:43:39 AM6/3/13
to materials-welding
Yes, QW200.4
Pandithan
Welding Consultant


--
To post to this group, send email to material...@googlegroups.com
To unsubscribe from this group, send email to materials-weld...@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
For more options, visit https://groups.google.com/groups/opt_out.
 
 

veera raghava kommisetti

unread,
Jun 2, 2013, 7:58:56 AM6/2/13
to material...@googlegroups.com
Yes in both the cases.
 

Code Interpretations

Interpretation: IX-86-23

Subject: Section IX, QW-200.4, QW-306, and QW-407.4

Date Issued: March 21, 1986

File: BC85-553

Question (1): A Procedure Qualification Record (PQR) for a single welded joint was qualified using 1/2 in. thick base metal. GTAW was used for the first 1/8 in., and SMAW for the remaining 3/8 in. Will this PQR support a Welding Procedure Specification (WPS) for deposited weld metal thicknesses of 1/4 in. and less using GTAW?

Reply (1): Yes.

Question (2): Will the PQR in Question (1) support a WPS for deposited weld metal thicknesses of 3/8 in. and less using SMAW?

Reply (2): Yes.

Question (3): Will the PQR in Question (1) qualify a WPS for first using SMAW on 3/8 in. and less deposited weld metal thickness followed by GTAW on 1/4 in. and less deposited weld metal thickness?

Reply (3): Yes.

Question (4): The welder who successfully welded the test coupon for the PQR in Question (1) is to be used to production weld. Is it necessary to qualify this welder so that he may use the WPS in Question (1) within the variables of QW-350?

Reply (4): No.

Question (5): Is it necessary to qualify this welder so that he may use the WPS in Question (2), where the WPS uses backing, within the variables of QW-350?

Reply (5): No.

Question (6): Is it necessary to qualify this welder so that he may use the WPS in Question (2) where the WPS does not have backing in a single welded groove?

Reply (6): Yes.

Question (7): Is it necessary to qualify this welder so that he may use the WPS in Question (3) in a single-welded joint?

Reply (7): Yes.

Question (8): Is the GTAW weld deposit of the PQR considered the backing for the SMAW?

Reply (8): Yes.