MT before or after PWHT?

146 views
Skip to first unread message

Urdiansyah

unread,
Oct 19, 2015, 12:42:29 AM10/19/15
to Materials & Welding

Dear Expert,

 

Currently I work at fabricator of Pressure vessel and Heat exchanger,

During Renewal ASME, AI question about MT shall be done before or after PWHT ?

Kindly  advice for this matter

 

Thank you for answered,

 

Best Regards,

Urdiansyah

Engineering PIC

PT.Daekyung Indah Heavy Industry

Cilegon Plant :

Jl. Australia II Kav. K1 Kawasan Industri (KIEC)

Cilegon 42443, Banten - INDONESIA 

Mohd Azam

unread,
Oct 19, 2015, 12:54:50 AM10/19/15
to material...@googlegroups.com

As a good engineering practice and Final product (After PWHT) shall be carried out MT 


Thanks 

Azam


--
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To post to this group, send email to material...@googlegroups.com.
Visit this group at http://groups.google.com/group/materials-welding.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/4c4f5ad7-fc11-4d20-a7c3-0ac84044a3b2%40googlegroups.com.
For more options, visit https://groups.google.com/d/optout.

Ramdoss Ravindiren

unread,
Oct 19, 2015, 2:11:23 AM10/19/15
to material...@googlegroups.com
Dear Azam,

It is bettter to do after PWHT, so that after  stresses are relieved, surface cracks can be detected, if any....

Regards
Ram

From: Mohd Azam
Sent: ‎19-‎10-‎2015 10:24 AM
To: material...@googlegroups.com
Subject: Re: [MW:23744] MT before or after PWHT?

Kannayeram Gnanapandithan

unread,
Oct 19, 2015, 2:11:25 AM10/19/15
to materials-welding
code does not say before or after for sec 8 construction, but it is good  engineering practice to MT before and after for P1 materials. As far as B31.1 power piping u have to do NDE after PWHT for materials P3,4,5,15E  

THANKS & BEST REGARDS,
KG.PANDITHAN, IWE,  AWS-CWI, CSWIP 3.1,
CONSULTANT-WELDING & QUALITY

--

Urdiansyah

unread,
Oct 19, 2015, 3:33:17 AM10/19/15
to Materials & Welding

Thank you for the answers,

I agree with your answer that commonly MT is done after PWHT.

But in some condition MT shall be done before PWHT,

Still looking for this condition? In which CODE

 

Thanks,

Urdi 

george....@gr.bureauveritas.com

unread,
Oct 19, 2015, 11:47:36 AM10/19/15
to Urdiansyah
After

Sent from my BlackBerry 10 smartphone.
From: Urdiansyah
Sent: Δευτέρα, 19 Οκτωβρίου 2015 - 07:42
To: Materials & Welding
Subject: [MW:23742] MT before or after PWHT?

--
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To post to this group, send email to material...@googlegroups.com.
Visit this group at http://groups.google.com/group/materials-welding.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/4c4f5ad7-fc11-4d20-a7c3-0ac84044a3b2%40googlegroups.com.
For more options, visit https://groups.google.com/d/optout.

This message contains confidential information. To know more, please click on the following link: http://disclaimer.bureauveritas.com

c sridhar

unread,
Oct 19, 2015, 11:47:36 AM10/19/15
to material...@googlegroups.com
It is like  whether RT to be done before or after PWHT. 
Similar to RT, prefer to do MT also prior to & post PWHT . 

Defects if any can be rectified  prior hand to avoid double 
PWHT. In fact, MT is much more economical compared to RT. 
We saved a lot following above sequence with Alloy steel 
welding in a petro- chemical project. But choice is yours.

C Sridhar.



 


From: Ramdoss Ravindiren <rdos...@gmail.com>
To: "material...@googlegroups.com" <material...@googlegroups.com>
Sent: Monday, 19 October 2015 10:49 AM
Subject: RE: [MW:23745] MT before or after PWHT?

Tadic, Miroslav

unread,
Oct 19, 2015, 12:56:08 PM10/19/15
to material...@googlegroups.com

Considering money in END final costs, and that MT is relativity cheap, you could use MT before and after PWHT

 

So, both examination can help you to verify any indication

 

That’s my recommendation and in your place, I schedule END in that way

 

Best regards

 

Miroslav Tadic
Integrity Enginner
CEE
Gerencia de Producción - Mantenimiento
YPFB Chaco S.A.

Jim Price

unread,
Oct 20, 2015, 12:41:42 AM10/20/15
to material...@googlegroups.com

Below information can be found on the National Board website.

 

http://www.nationalboard.org/index.aspx?pageID=164&ID=377

 

 

Advantages and Disadvantages of Using Magnetic Particle Examination

 

Advantages:

  • Can detect both surface and near-surface indications. 
     
  • Surface preparation is not as critical compared to other NDE methods. Most surface contaminants will not hinder detection of a discontinuity.
     
  • A relatively fast method of examination.
     
  • Indications are visible directly on the surface.
     
  • Low-cost compared to many other NDE methods.
     
  • A portable NDE method, especially when used with battery-powered yoke equipment.
     
  • Post-cleaning generally not necessary.
     
  • A relatively safe technique; materials generally not combustible or hazardous.
     
  • Indications can show relative size and shape of the discontinuity.
     
  • Easy to use and requires minimal amount of training.

 

 

Jim Price | Welding Engineer, CWI

Direct:  320.7463439 | Fax: 417-862-5564

jimp...@polarcorp.com

cid:image001.jpg@01D0E005.E9837830

 

 

 

 

Jim Price

unread,
Oct 20, 2015, 12:42:00 AM10/20/15
to material...@googlegroups.com

RT before PWHT is what one company, I know of performs and MT after PWHT.

I Googled to find the depth of flaw detection and below is the response I received.

(I thought it was 1/8” but wanted to find out for sure before responding.)

Q: What is the maximum depth that magnetic particles can detect a discontinuity? 
A: 1/4 inch, however 0.050 to 0.100 inch is a more realistic depth.

 

Detection will depend on current AC or DC and wet or dry.

 

Best Regards

 

Jim Price | Welding Engineer, CWI

Direct:  320.7463439 | Fax: 417-862-5564

jimp...@polarcorp.com

cid:image001.jpg@01D0E005.E9837830

 

 

 

 

 

From: material...@googlegroups.com [mailto:material...@googlegroups.com] On Behalf Of Tadic, Miroslav


Sent: Monday, October 19, 2015 11:00 AM
To: material...@googlegroups.com

Reply all
Reply to author
Forward
0 new messages