Does SS410S Weld overlay / butt welds (of SS 410S) requires PWHT?

278 views
Skip to first unread message

manohar matcha

unread,
Jun 14, 2014, 8:39:28 AM6/14/14
to materialswelding
Dear All,

Q1. Does SS 410S (E 410NiMo or ER 410NiMo) Weld overlay / clad restoration requires PWHT?
       WoL: Initial pass with E309L

Q2. Does SS 410S weld (butt) joints requires PWHT?
Regards,
Manohar.

Get your own FREE website, FREE domain & FREE mobile app with Company email.  
Know More >

S.Mohammed

unread,
Jul 30, 2014, 8:36:02 PM7/30/14
to material...@googlegroups.com
its depend whethet CRO done for strength purppse or corosion purpose.
for strength req
for corrosion not req.

Shridev Kurup

unread,
Aug 1, 2014, 1:22:36 AM8/1/14
to material...@googlegroups.com

Dear,

1.As per Sec ix 2013 table Qw/Qb 422 A/SA-240 Type 410s is P7 Gr-1 Uns no 41008 and if you go to ASME sec VIII div 1 3024 table UHA 32-2 P7 material required heat treatment. Holding temp 730 degree C. Upto 2 inch 1 hr/inch, 15 min minimum. More than 2 inch ,2 hr plus additional 15 min for every inch up to 5 inch.

If design code other than sec viii details may vary.

2.It depends on what Wps you are using as per welding code. PWHT is Essential veriable in most of the Wps  for CRO in Article 2 as per sec ix.

Regards
Shridev

> --
> To post to this group, send email to material...@googlegroups.com
> To unsubscribe from this group, send email to materials-weld...@googlegroups.com
> For more options, visit this group's bolg at http://materials-welding.blogspot.com/
> http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
>
> The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
> ---
> You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
> To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
> For more options, visit https://groups.google.com/d/optout.

Reply all
Reply to author
Forward
0 new messages