weld thickness

60 views
Skip to first unread message

Raghul

unread,
Aug 30, 2019, 2:53:08 PM8/30/19
to Materials & Welding
Background: A welder tests on an NPS 6 Sch. 80 (0.432 in. wall) coupon, depositing 0.100 in. of E6010 and the balance of 0.332 in. using E7018.

Question (1): Using E6010, is the welder qualified to deposit 0.864 in. maximum of weld metal?

Reply (1): Yes.

Question (2): Using E7018, is the welder qualified to deposit 0.664 in. maximum of weld metal?

Reply (2): Yes.

Question (3): Is the welder qualified to deposit 0.864 in. of weld metal using E6010 plus 0.664 in. of E7018 weld metal deposit thickness for a total of 1.528 in. in the same groove?

Reply (3): No

Above clauses are get from ASME ix interpretation.

Please explain  Using E6010, how the welder qualified to deposit 0.864 in. maximum of weld metal???????

Aakash

unread,
Oct 21, 2019, 9:36:40 AM10/21/19
to Materials & Welding
Interpretation number please

defrih...@gmail.com

unread,
Oct 22, 2019, 1:26:06 AM10/22/19
to Materials & Welding
All Answer : No
Because range qualification welder for production 2t, So E6010 max 0,2 Inch and E7018 max 0,664 Inch
refer to QW 451 ASME IX

Tajuddin Mohammed

unread,
Nov 7, 2019, 10:19:07 PM11/7/19
to material...@googlegroups.com
Please Refer QW-433 ASME Sec iX
1.If a welder qualified for F4 with backing can weld F3 with backing as per QW-433
Welder is already qualified for F3 without backing 0.200 inch max (2×0.100 inch) and One more 0.664 inch with F3 he can weld total 0.864 inch.

2. For thickness of weld metal qualified refer QW-452.1(b)
For example welder deposited F4 0.332 inch thickness weld metal deposited.
Maximum weld metal deposited will ne 2×0.332= 0.664.




Mohammed Tajuddin

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/495bdc6f-e17d-4882-a2a5-51aff73fb83c%40googlegroups.com.
Screenshot_20191107-200325_Drive.jpg
Screenshot_20191107-201000_Drive.jpg
Reply all
Reply to author
Forward
0 new messages