Dear Experts,


Good day.


Regarding the mentioned subject, we have done PWHT for 2” SCH XS socket joint caustic line. Job was in service piping based on MOC there was heat treatment requirement.


Now problem is that during PWHT cycle due to the power breakdown cycle was uncompleted.  Temperature were reached up to 610°C job was interrupted before starting the holding time.


As per that particular shift Inspector’s instruction job was restarted form 150°C and completed the job.


The next shift inspector is rejecting the job and asking to replace those particular fittings (elbows).


According to the above details, Please clarify is it acceptable multiple times of PWHT in the same weld joint or the fittings should be changed.


I hope that I have given enough details and looking for your valuable replies.


Thanks & Warm Regards,

KARTHIKEYAN  M.
P Save A Tree - Please do not print unless really need

Prakash Hegde

unread,
Feb 11, 2017, 9:38:37 PM2/11/17
to material...@googlegroups.com
Hi!
As per ASME code
What you have done is not objectionable as per ASME code
i.e. If the joint is not soaked as per code requirement at at rn such caseequired soaking temp.
In such case you can reheat and soak at required time and temp.
You can refere UCS 56 of ASME code
Regards
Hegde


--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To post to this group, send email to material...@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAL7K%3D_%2Bh%3DDFVC4OkDvq6k9XYJqU0fakDRppSnzrw2oko_UWSqg%40mail.gmail.com.
For more options, visit https://groups.google.com/d/optout.


Yasir Bhatti

unread,
Feb 11, 2017, 9:38:41 PM2/11/17
to material...@googlegroups.com
Karthick;

I have faced similar situation in P-15E ,happens once in a while the only possible potential is weldmet can softer after multiple sessions of stress relief. Propose as corrective action hardness of weld/base metal to be checked. If its less than base metal itself then you have to replace the assembly completely and if its near acceptable value then its fine.


Regards,

Yasir Ghous

--

muthu barathi

unread,
Feb 11, 2017, 9:38:54 PM2/11/17
to material...@googlegroups.com


Dear Sir,


what is moc and if it is cs no problem as you are carriedout PWHT


Thanking You.

With Warm Regards,

Muthu Barathi P.
Mobile : +9184695933

Sent from RediffmailNG on Android





From: Karthikeyan Muthuvel <m.karth...@gmail.com>
Sent: Sat, 11 Feb 2017 19:09:47 GMT+0530
To: "material...@googlegroups.com" <material...@googlegroups.com>
Subject: [MW:26041] Towice the PWHT for the same weld joints

Dear Experts,


Good day.


Regarding the mentioned subject, we have done PWHT for 2” SCH XS socket joint caustic line. Job was in service piping based on MOC there was heat treatment requirement.


Now problem is that during PWHT cycle due to the power breakdown cycle was uncompleted.  Temperature were reached up to 610°C job was interrupted before starting the holding time.


As per that particular shift Inspector’s instruction job was restarted form 150°C and completed the job.


The next shift inspector is rejecting the job and asking to replace those particular fittings (elbows).


According to the above details, Please clarify is it acceptable multiple times of PWHT in the same weld joint or the fittings should be changed.


I hope that I have given enough details and looking for your valuable replies.


Thanks & Warm Regards,

KARTHIKEYAN  M.
P Save A Tree - Please do not print unless really need

--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To post to this group, send email to material...@googlegroups.com.
To view this discussion on the web visit https:roups.google.com/d/msgid/materials-welding/CAL7K=_+h=DFVC4OkDvq6k9XYJqU0f...@mail.gmail.com.

K.M Hrishikesan

unread,
Feb 11, 2017, 9:39:03 PM2/11/17
to materials-welding
Establish a repair welding procedure by running a PQR with double PWHT cycle. This can regularise the thing and convince your inspector. 

--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAL7K%3D_%2Bh%3DDFVC4OkDvq6k9XYJqU0fakDRppSnzrw2oko_UWSqg%40mail.gmail.com.

George Dilintas

unread,
Feb 12, 2017, 7:29:02 AM2/12/17
to Meghanadh K
I would suggest to have a look on 124.2 of ASME B31.1-2016 before you conclude

To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
To view this discussion on the web visit https:roups.google.com/d/msgid/materials-welding/CAL7K=_+h=DFVC4OkDvq6k9XYJqU0fakDRppSnzrw2oko_...@mail.gmail.com.

For more options, visit https://groups.google.com/d/optout.

--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/1486820387.S.14981.24694.f5-224-116.1486823313.15194%40webmail.rediffmail.com.

For more options, visit https://groups.google.com/d/optout.



--
Dr. Georgios Dilintas,
Dipl. Ing. In Aeronautic and Space Engineering
Ph.D in Mechanics of Solids - Computational Mechanics
A.I.S, A.N.I, IRCA Lead Auditor
Welding, Stress Analysis, Corrosion, QA/QC, Failure Analysis, Risk Analysis