DENSITY OF RT FILM

96 views
Skip to first unread message

SEN SEN

unread,
Dec 2, 2021, 10:14:08 PM12/2/21
to MATERIAL
Dear experts
    while doing film interpretation, which all area need to be checked for density with densitometer? spec says 1.8 to 3.5, is it only for weld area or also for entire area of film

please clarify with  which code,
thanks with regards,
senthil P

SENTHILKUMAR SWAMINATHAN

unread,
Dec 3, 2021, 1:04:20 AM12/3/21
to material...@googlegroups.com
Worst area where IQI placed and Sensitivity achieved in that particular area
to 
Best area where IQI placed density check. 
where us densitiy range -15% to 30%

Thank you, 

Regards, 
S.SENTHILKUMAR


--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAGYkEe2ecsSUJVSKCTzo9H59mrMwKFSiMyNz87NHu9Gq3cL3sw%40mail.gmail.com.

Muhammad Azeem

unread,
Dec 3, 2021, 4:17:49 AM12/3/21
to material...@googlegroups.com
Hi senthil,
You just need to checked the area of concern weld only. Any defect withing the weld area will be consider as film defect as Reshoot or weld defect in case of reject or accept within limitations. 


Asme sec V for Non destructive testing. 



Adriaan Stoltz

unread,
Dec 6, 2021, 11:34:24 PM12/6/21
to material...@googlegroups.com

Area of interest should be weld and HAZ, density must be acceptable for both areas.

Mhaskar Aly

unread,
Dec 9, 2021, 10:39:20 PM12/9/21
to material...@googlegroups.com
You need to check density on IQI..from that reading you get tolerance of plus 30% and  minus 30%. Minimum 1.8 and maximum 4 (For Xray).

Suppose you get density on IQI as 2.1 then add 30%  and minus 15%; your range will be 1.8 to 2.73%.

Density of all areas of interest shall be within that range. 1.8 to 2.73 ( not 4).