I have to qualify a PQR in following conditions

Construction Code AWS D1.1
Material API 5L Gr B
Welding position 6GR
Base material
Diameter 6"
Thickness on none bevel end = 14.27 mm
Thickness on bevel end = 7.11 mm

Query

1.  What should be the thickness Range for WPS without CVN testing ?

2.  What should be the thickness Range for WPS with CVN testing ?

Looking forward for support with Clause reference if possible.

Regards,
Prashant

hoàng nguyễn

unread,
Nov 30, 2019, 10:23:22 AM11/30/19
to material...@googlegroups.com
1. Thickness Range for WPS without CVN testing: 3 mm to 14.22 mm
2. Thickness Range for WPS with CVN testing: 7.11 mm to 14.22 mm (Refer to Table 4.6 ( 2)).
Refer to Table 9.10.

Vào Th 2, 4 thg 11, 2019 vào lúc 10:14 Prashant <pprane...@gmail.com> đã viết:
--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/e69784e4-8b80-4771-9637-93466f43f84b%40googlegroups.com.
Reply all
Reply to author
Forward
0 new messages