Group number selection when toughness requirement is there

57 views
Skip to first unread message

praba karan

unread,
Feb 6, 2026, 3:53:40 AMFeb 6
to Materials & Welding
Dear Experts,

Need your clarification on the following,

When the PQR(GTAW+SAW) is qualified with (Pno-1 Group no 1) with (Pno-1 Group no 2).-With impact test.

As per Sec IX, G number will be essential variable when toughness requirement is there, So can i prepare WPS for the same p number and same group number within themselves?
Like, 1)  Pno1, Group no 1 to Group no 1
          2)  Pno1, Group no 2 to Group no 2,

or is there any other suggestions to cover all groups?

Thank you..

dia shukr

unread,
Feb 6, 2026, 4:07:20 AMFeb 6
to material...@googlegroups.com
Dear

If you have toughness test in this case you shall quilefy group number 1 with group number 2 and as ASME IX this will qualify G1to G2. G1 to G1 and also G2 to G2. For example if you have pipe(G1) and fitting (G1) and you have flange(G2) is not accepted to qualify pipe to fitting but the correct way is to weld pipe with flange or fitting with flange for procedure qualification.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To view this discussion visit https://groups.google.com/d/msgid/materials-welding/90d39d5b-a8b3-4492-953d-c766aa71432en%40googlegroups.com.

Cezar Varin

unread,
Feb 6, 2026, 4:21:47 AMFeb 6
to material...@googlegroups.com
Hi,

You can input in your WPS like below

P. No.1 Gr. No. 1&2 to P. No.1 Gr. No. 1&2

and it will cover all.

Thanks!


Hai Tran Ngoc

unread,
Feb 6, 2026, 5:02:41 AMFeb 6
to material...@googlegroups.com

Hi,

You already have a PQR for P1 Group 1 with P1 Group 2, and you performed an impact test.
According to ASME IX - QW 403.5, you can make the WPS as follows:

  1. P-No.1 Gr.1 with P-No.1 Gr.1
  2. P-No.1 Gr.2 with P-No.1 Gr.2
  3. P-No.1 Gr.1 with P-No.1 Gr.2

Or you can combine them like this:
P-No.1 Gr.1,2 to P-No.1 Gr.1,2


image.png


 

Hai, Tran Ngoc

E-mail: ngoch...@gmail.com
Tel.: +84-(0)977-881-880



Vào Thứ 6, 6 thg 2, 2026 vào lúc 16:21 Cezar Varin <cezar...@gmail.com> đã viết:

dia shukr

unread,
Feb 6, 2026, 5:02:41 AMFeb 6
to material...@googlegroups.com
Dear 

In this case your material MTC should achieve both group (G1&G2)  for example some times we receive material like ASTM A516 achieve both groups (grade 65&70) in this case you can write in the WPS group 1&2 to group 1&2. Otherwise you have to qualify G1 to G2.



Birupakhya Sahu

unread,
Feb 6, 2026, 5:02:41 AMFeb 6
to material...@googlegroups.com
Yes , It is acceptable with G1 to G1 & G2 to G2 subject to HAZ Impact test required to perform for both HAZ G1 & G2 in PQR.

Regards,
Birupakhya Sahu
TEMA India Private Limited, 
Kherdi, Silvassa (D&NH).



--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To view this discussion visit https://groups.google.com/d/msgid/materials-welding/90d39d5b-a8b3-4492-953d-c766aa71432en%40googlegroups.com.



________________________________________________________________________________________________________________________________
This email (including any attachment(s) hereto) contains confidential or privileged information intended solely for the designated individual or entity to whom it is addressed. If you are not the intended recipient, please delete this message permanently and notify the sender immediately. Any unauthorized use, disclosure or distribution is strictly prohibited. TEMA India Pvt Ltd is not liable for the improper transmission of this message or any damage sustained as a result of it.
________________________________________________________________________________________________________________________________

james gerald

unread,
Feb 6, 2026, 5:20:33 AMFeb 6
to 'Birupakhya Sahu' via Materials & Welding
Snap shot from ASME Sec.IX
Inline image


Thanks & Regards

J.Gerald Jayakumar

0091-8838619635



praba karan

unread,
Feb 6, 2026, 5:44:49 AMFeb 6
to Materials & Welding
Dear's

Thanks for the better clarification.