Suitable filler wire for UNS S13800/ ASTM-A 705 Gr XM-13 PH 13-8 Material

163 views
Skip to first unread message

Prem Nautiyal

unread,
Apr 18, 2021, 11:20:47 PM4/18/21
to material...@googlegroups.com
Dear All

We need expert advice on best  suitable filler wire and Welding process for following base  material - 

Base Material :  AISI/ UNS S13800/ ASTM-A693/ A 705 Gr XM-13  PH 13-8
   
Chemical Requirements of base material: 

Carbon 0.05 
Manganese 0.2 
Phosphorus 0.01
Sulfur 0.008
Silicon 0.1
Chromium 12.25 to 13.25
Nickel 7.5 to 8.5
Aluminum  0.9 to 1.35
Molybdenum 2 to 2.5


  Base material thickness 8 to 16mm thk..  
   
  1)  Welding Process :  TIG or SMAW
   
  2) Joint geometry : Butt Weld (Full penetration joint)  
  3) Age hardening to be done after welding  
  4) After age hardening UTS shall be 1520 Mpa min, YS = 1420 MPa, El= 10%.  
  5) After age hardening hardness required 45 HRC minimum  


We have selected one TIG filler wire Turballoy 13-8 Mo which matches the chemical composition of our base material and has same UNS Number. The manufacturer is United States Welding Corporation but not available in India..

We have past experience of 15-5 PH stainless steel welded with ER 630 Filler wire but UTS achieved after age hardening is 1100 MPa.

Also some reputed consumable manufacturers have suggested ER 630 filler wire but cannot guarantee strength and hardness after age hardening.


We would like to know the suitable filler wire / electrode and best process to weld this material - TIG / SMAW.

Regards


Prem Nautiyal 

Cell 9082354678 / 9082354678


Prem Nautiyal

unread,
Apr 20, 2021, 11:00:50 PM4/20/21
to material...@googlegroups.com

pgos...@rogers.com

unread,
Apr 20, 2021, 11:44:07 PM4/20/21
to material...@googlegroups.com, prem.na...@gmail.com

Hi Prem,

 

These alloys are really special type of alloys. Precipitation hardenable hence all alloys have to be aged after welding . Different aging temperatures are applicable according to the specifications and required properties. I’ve highlighted the nominal mechanical properties in SA-564 ,extract as attached.

Typically, E 630 electrodes/filler metals are used for welding 17/4ph stainless steel. This grade is most commonly used PH stainless steels , in valves and other components.

If matching Turballoy 13-8 welding consumable is not available by any means, 17/4 ph or E/ER 630 electrode/filler metal would be the way to go.

 

If E630 does not meet the criteria, consumables for Precipitation hardenable Nickel Based alloys would be the only available  option.

 

Regards.

 

Pradip Goswami.P.Eng, IWE.

Independent  & Consulting Welding & Metallurgical Specialist

Linkedin: https://www.linkedin.com/in/pradip-goswami-2999855/

Email:pgos...@rogers.com,pradip....@gmail.com

Cell/Whasapp:1-905-9793232

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAEP2HKAc6iCuSmTNzPBmzM4Je1Krwd8O2Z%2B-%3DAqJ3Kz7rmQeKA%40mail.gmail.com.