How to calculate Repair percentage

2,051 views
Skip to first unread message

Karuppa Samy

unread,
Oct 9, 2023, 2:54:58 AM10/9/23
to Materials & Welding
Dear experts,

how to calculate radiography repair percentage for 100% RT joints and random RT joints. please explain with applicable reference standard

Babur Khan

unread,
Oct 10, 2023, 3:42:07 AM10/10/23
to material...@googlegroups.com
Greetings
Below here is repair rate farmula 

% RR = (Lr/ Lw) X 100
where:
% RR = percent repair rate.
Lr = welder's total length of repairs in one week, mm
Lw = welder's total length of weld radiographed in one week, mm

Muhammad Babur Khan

Sent from my iPhone

On 9 Oct 2023, at 9:54 AM, Karuppa Samy <samy...@gmail.com> wrote:

Dear experts,

how to calculate radiography repair percentage for 100% RT joints and random RT joints. please explain with applicable reference standard

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/855522fb-714e-4f59-916f-da475471e4b2n%40googlegroups.com.

james gerald

unread,
Oct 10, 2023, 3:42:08 AM10/10/23
to material...@googlegroups.com
The repair percentage for 100% RT Joints may be calculated by the below 3 methods as recommended in the Client Specification.

1. Joint Wise - Number of Joints Defective / Total Number of Joints Radiographed x 100
2. RT Film Wise - Number of Repair Films / Total Number of Films Radiographed x 100
3. Length Wise  - Length of Repair / Total Length Radiographed x 100

Acceptance Limits as per Client Specification.

Random RT depends on Applicable Code + Client specification.

Example of ASME B31.3 as below.

Inline image

Penalty for defective Joints as per Applicable Client Specification.

Thanks & Regards

J.Gerald Jayakumar



On Monday, 9 October, 2023 at 12:24:52 pm IST, Karuppa Samy <samy...@gmail.com> wrote:


Dear experts,

how to calculate radiography repair percentage for 100% RT joints and random RT joints. please explain with applicable reference standard

--

DOMINIC V.K

unread,
Oct 12, 2023, 12:37:34 AM10/12/23
to material...@googlegroups.com
It's client (End of User) requirements. For example Contactor shall deploy Welders with previous qualification records with proven performance of statistical repair rate less than 3% and continuity of Welding within 6 months. (Number of joints repair/Total Radiographed X 100)
Normally industry practices keep it with in 3% repair rate.