SS 310 TO SS 316 & SS316 TO SS304 Welding joint qualification & filler wire

472 views
Skip to first unread message

Soumen Samanta

unread,
Mar 2, 2024, 4:27:52 AM3/2/24
to Materials & Welding
Dear Expert,

We have PQR base metal SS304 TO SS304 & filler wire ER 308L 
I have the following question 
1)Can we weld SS310 TO SS316 with the above pqr and what will be the filler for the same?
2)Can we weld SS316 TO SS304 with the above pqr and what will be the filler for the same?


Thanks in advance

Sahil musani

unread,
Mar 4, 2024, 9:37:47 PM3/4/24
to material...@googlegroups.com
PQR Base metal SS304 (P8, Gr.1) TO SS304 (P8, Gr.1) & filler wire ER 308L (F No.6, A No.8)

ANS. 1) Yes you weld SS310  (P8, Gr.2) TO SS316  (P8, Gr.1) with the above PQR, Filler you have two options: ER310 or ER309.
ANS. 2) Yes you weld SS316  (P8, Gr.1) TO SS304  (P8, Gr.1) with the above PQR, Filler you have two options: ER308L or ER316L.

{Note: Your minimum design metal temperature shall not be colder than –155°F (–104°C)}

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/33355d65-cf1b-48c3-bab5-3c223407725an%40googlegroups.com.


--
Regards,
Sahil Musani

Parminder Singh

unread,
Mar 5, 2024, 12:51:06 AM3/5/24
to material...@googlegroups.com
Find attached the following answers: 

1)Can we weld SS310 TO SS316 with the above pqr and what will be the filler for the same? 

No, you have to requalify the PQR as A No. Change from 8 to 9. 
Filler: SS310

2)Can we weld SS316 TO SS304 with the above pqr and what will be the filler for the same?

Yes, if Impact is not applicable. 

--

Kannayeram Gnanapandithan

unread,
Mar 5, 2024, 12:51:06 AM3/5/24
to materials-welding

Sahil musani

unread,
Mar 5, 2024, 9:47:28 AM3/5/24
to material...@googlegroups.com
Yes, Parminder singh & Kannayeram sir are right,sorry my mistake Filler: SS310 A no. is 9.