Hello good evening all experts
Can we use E71T1-1C-H4/H8 AWS SFA 5.36 filler wire instead of E71T1-1C-H4/H8 AWS SFA 5.20 if yes then please send me any  reference from code and standard by ASME-2C or SEX 9 or SAES- W12 or W11 or any international standard because our WPS is qualified on AWS 5.20 but we recieved Consumable material AWS SFA 5.36.         This attached label is recieved material 

Regards ,
Zafar 
00966544639978 
IMG-20210929-WA0059.jpg

Vishwas Keskar

unread,
Sep 29, 2021, 11:43:16 PM9/29/21
to material...@googlegroups.com
PQR qualified  with SFA no XXXX , same shall be used in production Welding.

Now 2021 edition 5.36 is withdrawn. 

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAP9k9XfupDcLPwdc9kiJyUMxaU%2Bhz%3DHr13PVMmsgj_bO%3Dy_OEw%40mail.gmail.com.

Kannayeram Gnanapandithan

unread,
Sep 30, 2021, 1:50:52 AM9/30/21
to materials-welding
SFA no is not essential, only Fno & Ano is essential

THANKS & BEST REGARDS,
KG.PANDITHAN, BE, IWE,  CSWIP 3.1,
ISO 9712 Level 2 in VT,
ASNT-Level II in PT,MT,RT & UT,
LA ISO 9001-2015,
International Welding Engineer. 
CONSULTANT-WELDING & QUALITY
Mobile no: +919940739349


--

james gerald

unread,
Sep 30, 2021, 4:00:54 AM9/30/21
to material...@googlegroups.com
There are 3 points to be considered as experts mentioned as below.

1. In ASME 2021 edition SFA 5.36 has been discontinued but I suppose the recalled may be used based provided the welding consumable certificate matches with A-Number of that Qualified for PQR.
 
2. Both SFA 5.20 & SFA 5.36 falls under F-Number 6 & hence  no issue.

3. Ensure the Shielding gas as qualified for 100%Co2