Facing crack in during overlay welding of Stellite 12 on Duplex material

326 views
Skip to first unread message

SURESH

unread,
Nov 20, 2020, 4:46:41 AM11/20/20
to Materials & Welding
Dear Experts
During welding of Duplex grade material we are facing crack on the weld metal as attached in the photo. Below is the detailed process for reference

Process: PTAW
Base Material: ASTM 182 Gr.F55
Consumable: Stellite 12 (Powder)
PreHeat: Nil
Interpass: <200*C
Current: 128 to 145
Gas: Ultra Pure ARGON
Job Size: OD544 X ID 472 X Thk 36mm
Welding: Overlay weld on OD Surface alone


We are welding deposition thickness of 3mm. So as per this we are doing welding of 2 layer with multi pass, On welding second layer we found crack. Can anyone suggest where it is went wrong and why this crack is propagated. Please advice

 

In First layer- Total of 12 weld pass

In second layer- Total of 12 weld pass



Regards

Suresh

Raghuram Bathula

unread,
Nov 20, 2020, 4:53:45 AM11/20/20
to Materials-Welding

Srinivasan Jagannathan

unread,
Nov 20, 2020, 6:17:34 AM11/20/20
to material...@googlegroups.com
Dear Suresh

Are you getting the crack during the deposition? Or after the job is cooled?

Srinivasan

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/8fd110ad-c422-4025-bf91-632d75b53a60n%40googlegroups.com.


--
J.SRINIVASAN
Mobile : 75501 82117



SURESH

unread,
Nov 20, 2020, 11:07:36 AM11/20/20
to Materials & Welding
Dear sir
While welding itself I am getting crack.

Ring is holded in the positioner by means of clamps at 90 degree and we are proceeding the welding.


Regards
Suresh

d...@btinternet.com

unread,
Nov 20, 2020, 11:07:47 AM11/20/20
to material...@googlegroups.com, d...@btinternet.com

Stellite12 deposits are prone to cracking due to local residual stress and limited ductility.

Thus, preheat has to be applies in order to minimise this susceptibility.

Sincerely,

David Harvey, 20 11 2020.


D Harvey, Director & Welding Metallurgist,
Eclipse Welding Metallurgy & Associates,
d...@btinternet.com
07768 004701
ONC, HNC, LIM, BSc, PhD.
Gas Turbine Industries: Civil, Military, Industrial, Power & Marine.

Memberships: AWS, AWD, ASM, TWI, IOM3,

Srinivasan Jagannathan

unread,
Nov 20, 2020, 11:39:56 AM11/20/20
to material...@googlegroups.com
Dear Suresh,
Grind the surface just before the deposition and try. This might be due to Chromium oxide which has already formed on the surface. Also slow cool by wrapping the entire job with an asbestos cloth.

Srinivasan  


Vanchinath S.A.

unread,
Nov 21, 2020, 3:41:59 AM11/21/20
to material...@googlegroups.com
Nickel barrier maybe required for stellite deposit on duplex steel. 
Vanchinath

pgos...@rogers.com

unread,
Nov 21, 2020, 11:35:42 PM11/21/20
to material...@googlegroups.com

ASTM 182 Gr.F55 is Zeron 100 forged product. The base metal hardness could be anything close to 28HRC or less. It’s reasonably high hardness value. Although PTAW is widely followed  for depositing Stellite overlay, it could embrittle Duplex , if the heat input is high. What is the Preheat temperature(if at all) adopted, and the  calculated Heat Input. For Zeron 100, Q should be typically 1.0-12.Kj/mm.

In your,  case the cracks are visible after depositing 2nd layer(i.e. Stellite  over Stellite), which is an indicator that hard products like Stellite are not able to accommodate the shrinkage  stress. In case of Stelllite  hardfacing application of buffer layers with Nickel base alloys(Alloy 625) could be of help.

Refer the provided guidance in this literature as a reference.

 

Thanks.

P.Goswami.P.Eng, IWE.

Independent  & Consulting Welding & Metallurgical Specialist

Linkedin: https://www.linkedin.com/in/pradip-goswami-2999855/

Email:pgos...@rogers.com,pradip....@gmail.com

Cell/Whasapp:1-905-9793232

Stellite Deposition onto Steel Substrates-General Guidelines.pdf