Support Welding of Cladded Pipes

58 views
Skip to first unread message

Biplab Pal

unread,
Jun 11, 2016, 10:34:00 PM6/11/16
to materials-welding
Dear Experts,

We have the Cladded Pipe of ASTM A335 Gr P11 (9.3 mm to 25 mm)  with internally cladded with SS347 (3mm).

We need to weld the Pipe Support with the pipes.

Our pipe support is P11 grade and the WPS is qualified with PWHT @740 for minimum 2 hours.

If we do PWHT is it going to effect the SS cladding? is there any corrosion issue.

We need your kind advice.

--
Thanks & Regards
Biplab Pal
Welding Inspector
E-mail:   bipla...@gmail.com
 
Information in this email and any attachments is confidential and intended solely for the use of the individual(s) to whom it is addressed or otherwise directed. Please note that any views or opinions presented in this email are solely those of the author and do not necessarily represent those of the Company. Finally, the recipient should check this email and any attachments for the presence of viruses. Myself accepts no liability for any damage caused by any virus transmitted by this email.
 

M.Sathiya Narayanan

unread,
Jun 12, 2016, 1:33:31 AM6/12/16
to material...@googlegroups.com
the corrosion property will deteriorate to some extent based on the PWHT control, 

as SS 347 is stablized one deterioration  will be limited to some extent 

WPS shall be qualified on cladded plate with PWHT and corrosion test on cladded area after PWHT  to ensure corrosion property  

--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To post to this group, send email to material...@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAFnzQg2_KsLhkjO679d_%3DfmBGrk_LD1J_yRKUETXr%2B2MP_OCVg%40mail.gmail.com.
For more options, visit https://groups.google.com/d/optout.



--
Thanks and Regards
M.Sathyanarayanan

dili...@gmail.com

unread,
Jun 13, 2016, 6:55:44 AM6/13/16
to 'Biplab Pal' via Materials & Welding
I assume the support will be attached by means of a fillet weld.
What is the throat size? You may do not need PWHT

Sent from my BlackBerry 10 smartphone.
From: 'Biplab Pal' via Materials & Welding
Sent: Κυριακή, 12 Ιουνίου 2016 - 05:34
To: materials-welding
Subject: [MW:24936] Support Welding of Cladded Pipes

--

Andreas Suryanda

unread,
Jun 15, 2016, 7:01:50 AM6/15/16
to Materials & Welding
I have several experience at clad material especially SS and Nickel Alloy material.
Basically, i believe PWHT at 740 is refer to the carbon steel and not intended to be done on clad material.
For clad material, you have to proof by mechanical test, chemical analysis.
However, since clad material is intended for corrosion resistance result, you may need to check for intergranullar corrosion on the clad material.
Personally I just PWHT for nickel clad material. And it seems affect the intergrannular corrosion resistance.

Regards,
Andreas Suryanda