Dear experts, 
Please clarify for impact test requirements of below variables.
Construction code ASME B31.3
Material A106 Gr. B
The thickness of Pipe. 17.48 mm
Temperature Limit 0^ F (-17.78^ C)
PWHT yes.
Table A-1 refers to curve B
Table 323.2.2A minimum Temperature without Impact Testing for CS showing under curve B 9^ F ( 12.8^ C).
My Question is for above case Impact testing for WPS qualification is required?  

Regards,

Muhammad Babur Khan Lashari
Sr. QA/QC Inspector (Welding)

(CSWIP 3.1 / CWI II From PWI) 

Mob: + 966 58 2774568 / 050 5193275

PAK : + 92 334 6186285 (Whatsapp)

Skype: babur.lashari

Sudhakar Kuppuswamy

unread,
Jul 31, 2019, 4:25:31 AM7/31/19
to google welding

In my opinion, for the below stated conditions, as per ASME B31.3, Impact test is applicable. I.e. supplementary essential variables for ASME Section 09 becomes essential variables. 

And, the qualified WPS thickness shall be T/2 to T+6mm, i.e. 8.74 mm to 23.48 mm in your case.


Regards,

Sudhakar K

Welding Engineer 




--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAN53wK1Vs8CgXP0uzAFyPAUNQ-gbaeg7axU9zRQZsXhV9p19jg%40mail.gmail.com.

pradip kumar Sil

unread,
Aug 1, 2019, 12:19:56 AM8/1/19
to materials-welding
Can you pls give reference for qualification thickness in this case



Babur Khan

unread,
Aug 1, 2019, 6:31:25 AM8/1/19
to material...@googlegroups.com
Dear Mr. Kumar,
Base metal thickness is 3.73 to 17.48mm


Muhammad Babur Khan
Sent from my iPhone

Sudhakar Kuppuswamy

unread,
Aug 1, 2019, 6:31:28 AM8/1/19
to google welding

You may please refer to Table 323.3.1 Impact Testing Requirements for Metals of ASME B31.3, Chapter 3.


Below is the snapshot, Refer A.5 


 

image.png


Regards,

Sudhakar K

Welding Engineer


حرف راز

unread,
Aug 2, 2019, 4:04:12 AM8/2/19
to material...@googlegroups.com
Dear sudhakar k,
very good reference but how can you relate this to WPS 

Khaled lamraoui

unread,
Aug 2, 2019, 4:04:12 AM8/2/19
to Materials & Welding
Dear experts. I need your help please. I have sa 335 p91 as base material used in power plant does this require impact test for preparation of pQR or not? Ps: used for high temperature applications 600 degree. Can you please give a detailed explanation. Khaled lamraoui.

anand gupta

unread,
Aug 2, 2019, 9:54:58 AM8/2/19
to material...@googlegroups.com, Khaled lamraoui
As per code for high temp impact test no need. 
Impact need for low temp only. 

Regards 
On Fri, 2 Aug 2019 at 13:34, Khaled lamraoui
Dear experts.    I need your help please.  I have sa 335 p91 as base material used in power plant does this require impact test for preparation of pQR or not?        Ps: used for high temperature applications 600 degree. Can you please give a detailed explanation.              Khaled lamraoui.         
--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsub...@googlegroups.com.

To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/88a57bae-9e31-4ebc-8c66-1ec9124eb25f%40googlegroups.com.

Dinesh Somwanshi

unread,
Aug 2, 2019, 9:55:00 AM8/2/19
to materials-welding
Dear sir,

Impact testing Its based on Mean design temperature cycle defined in drawing & If any project specs.

Thanks & Regards

DINESH VITTHAL SOMWANSHI

BACHELOR IN MECHANICAL ENGINEER

असो द्यावी दया तुमच्या लागतसे पाया.

*Pray for others, sometime, You might never need to pray for yourself
again.....*



Kannayeram Gnanapandithan

unread,
Aug 2, 2019, 12:02:52 PM8/2/19
to materials-welding
Check consumables are impact tested at room temperature. That's enough

To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/194641271.359695.1564750983528%40mail.yahoo.com.
Reply all
Reply to author
Forward
0 new messages