Need your guidance on the following:

We have tube to tube-sheet joint having Groove + Fillet Weld without grooves & expansion. (Tube-2.7mm, Tubesheet-45mm, P No.43 to P. No.43)

I have PQR qualified on plate 10mm Thk. (P No.43 to P No.43, Qualification Range - 1.5 to 20mm).

Can I use the same WPS for this joint or we have to qualify new procedure.

Procedure qualified as per ASME Sec.IX.

Need clarification with reference to clause number.

Neilashkumar

unread,
Nov 12, 2016, 2:15:00 AM11/12/16
to material...@googlegroups.com
No you cannot use plate WPS for tube to tube sheet . Your question seems irrelevant.

Need separate qualification for tube sheet.

P.NEILASHKUMAR 
Sent from my iPad
MOB : 966 551094590
             +91 9952110791
--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To post to this group, send email to material...@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/a0bf2487-921c-40df-a1f4-cc6886e07182%40googlegroups.com.
For more options, visit https://groups.google.com/d/optout.

Vanchinath S.A.

unread,
Nov 12, 2016, 5:17:03 AM11/12/16
to material...@googlegroups.com

Mock up qualification as per section IX with ten tubes required. Additionally pull test is to be done.


--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.

prem_nautiyal26

unread,
Nov 12, 2016, 9:56:21 PM11/12/16
to material...@googlegroups.com
Hi

Assuming your construction code is ASME SEC VIII div.1, 
You will have to carry out a separate tube to tube sheet mock up qualification.
Refer ASME SEC IX and SEC VIII Div 1 for details.
Also tube to Tube sheet mock up qualification will be mentioned in your approved QAP



REGARDS


PREM NAUTIYAL 
9769316004






Sent from my Samsung Galaxy smartphone.

-------- Original message --------
From: pankaj phuse <pankaj...@gmail.com>
Date: 11/11/2016 16:15 (GMT+05:30)
To: Materials & Welding <material...@googlegroups.com>
Subject: [MW:25662] Tube to Tubesheet Joint

Dear Experts,

Need your guidance on the following:

We have tube to tube-sheet joint having Groove + Fillet Weld without grooves & expansion. (Tube-2.7mm, Tubesheet-45mm, P No.43 to P. No.43)

I have PQR qualified on plate 10mm Thk. (P No.43 to P No.43, Qualification Range - 1.5 to 20mm).

Can I use the same WPS for this joint or we have to qualify new procedure.

Procedure qualified as per ASME Sec.IX.

Need clarification with reference to clause number.

--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To post to this group, send email to material...@googlegroups.com.

George Dilintas

unread,
Nov 13, 2016, 8:30:56 AM11/13/16
to Meghanadh K
Taking into account that your Pno is 43 you may benefit of the provisions of  QW 202.4.
However before take a final decisions check the requirements of QW 202.6

To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.

--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/3vk1jfblmfkop6qg13yd2on8.1478960138453%40email.android.com.

For more options, visit https://groups.google.com/d/optout.



--
Dr. Georgios Dilintas,
Dipl. Ing. In Aeronautic and Space Engineering
Ph.D in Mechanics of Solids - Computational Mechanics
A.I.S, A.N.I, IRCA Lead Auditor
Welding, Stress Analysis, Corrosion, QA/QC, Failure Analysis, Risk Analysis

Pravin Nimbalkar

unread,
Nov 13, 2016, 9:21:55 PM11/13/16
to Materials & Welding
Yes!

As per QW 202.6
Refer to QW 202.4 advantage for P No 43
(If construction code not refers QW193)

Regards,
Pravin Nimbalkar
Welding engineer
Bilfal heavy industries ltd. KSA
+966577620240

John Henning

unread,
Nov 14, 2016, 2:07:07 PM11/14/16
to material...@googlegroups.com

Minor adjustment - ASME Section VIII Div. 1 does not mandate tube-to-tubesheet mockup for qualification  - however Division 2 does.

 

From: material...@googlegroups.com [mailto:material...@googlegroups.com] On Behalf Of George Dilintas
Sent: Sunday, November 13, 2016 7:28 AM
To: Meghanadh K
Subject: Re: [MW:25676] Tube to Tubesheet Joint

 

Taking into account that your Pno is 43 you may benefit of the provisions of  QW 202.4.

However before take a final decisions check the requirements of QW 202.6

2016-11-12 16:23 GMT+02:00 'prem_nautiyal26' via Materials & Welding <material...@googlegroups.com>:

Hi

 

Assuming your construction code is ASME SEC VIII div.1, 

You will have to carry out a separate tube to tube sheet mock up qualification.

Refer ASME SEC IX and SEC VIII Div 1 for details.

Also tube to Tube sheet mock up qualification will be mentioned in your approved QAP

 

 

 

REGARDS

 

 

PREM NAUTIYAL 

9769316004

 

 

 

 

 

 

Sent from my Samsung Galaxy smartphone.

-------- Original message --------

From: pankaj phuse <pankaj...@gmail.com>

Date: 11/11/2016 16:15 (GMT+05:30)

To: Materials & Welding <material...@googlegroups.com>

Subject: [MW:25662] Tube to Tubesheet Joint

 

Dear Experts,

 

Need your guidance on the following:

 

We have tube to tube-sheet joint having Groove + Fillet Weld without grooves & expansion. (Tube-2.7mm, Tubesheet-45mm, P No.43 to P. No.43)

 

I have PQR qualified on plate 10mm Thk. (P No.43 to P No.43, Qualification Range - 1.5 to 20mm).

 

Can I use the same WPS for this joint or we have to qualify new procedure.

 

Procedure qualified as per ASME Sec.IX.

 

Need clarification with reference to clause number.

 

--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.

To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To post to this group, send email to material...@googlegroups.com.

--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.

To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To post to this group, send email to material...@googlegroups.com.



 

--

Dr. Georgios Dilintas,

Dipl. Ing. In Aeronautic and Space Engineering

Ph.D in Mechanics of Solids - Computational Mechanics

A.I.S, A.N.I, IRCA Lead Auditor

Welding, Stress Analysis, Corrosion, QA/QC, Failure Analysis, Risk Analysis

--

http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.

To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To post to this group, send email to material...@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAPOi40CvE1uMPy%3D9tkh3nNYYM1LCpvxobZhbQWbZivqGgJXMXA%40mail.gmail.com.

Shaunak Upadhyay

unread,
Nov 14, 2016, 10:33:48 PM11/14/16
to material...@googlegroups.com

No. You cannot use 10.0mm PQR for tube to tubes heel joint.


On 15 Nov 2016 02:07, "John Henning" <jhen...@deltak.com> wrote:

Minor adjustment - ASME Section VIII Div. 1 does not mandate tube-to-tubesheet mockup for qualification  - however Division 2 does.

 

From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of George Dilintas
Sent: Sunday, November 13, 2016 7:28 AM
To: Meghanadh K
Subject: Re: [MW:25676] Tube to Tubesheet Joint

 

Taking into account that your Pno is 43 you may benefit of the provisions of  QW 202.4.

However before take a final decisions check the requirements of QW 202.6

2016-11-12 16:23 GMT+02:00 'prem_nautiyal26' via Materials & Welding <materials-welding@googlegroups.com>:

Hi

 

Assuming your construction code is ASME SEC VIII div.1, 

You will have to carry out a separate tube to tube sheet mock up qualification.

Refer ASME SEC IX and SEC VIII Div 1 for details.

Also tube to Tube sheet mock up qualification will be mentioned in your approved QAP

 

 

 

REGARDS

 

 

PREM NAUTIYAL 

9769316004

 

 

 

 

 

 

Sent from my Samsung Galaxy smartphone.

-------- Original message --------

From: pankaj phuse <pankaj...@gmail.com>

Date: 11/11/2016 16:15 (GMT+05:30)

To: Materials & Welding <materials-welding@googlegroups.com>

Subject: [MW:25662] Tube to Tubesheet Joint

 

Dear Experts,

 

Need your guidance on the following:

 

We have tube to tube-sheet joint having Groove + Fillet Weld without grooves & expansion. (Tube-2.7mm, Tubesheet-45mm, P No.43 to P. No.43)

 

I have PQR qualified on plate 10mm Thk. (P No.43 to P No.43, Qualification Range - 1.5 to 20mm).

 

Can I use the same WPS for this joint or we have to qualify new procedure.

 

Procedure qualified as per ASME Sec.IX.

 

Need clarification with reference to clause number.

 

--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.

To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.

--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.

To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.



 

--

Dr. Georgios Dilintas,

Dipl. Ing. In Aeronautic and Space Engineering

Ph.D in Mechanics of Solids - Computational Mechanics

A.I.S, A.N.I, IRCA Lead Auditor

Welding, Stress Analysis, Corrosion, QA/QC, Failure Analysis, Risk Analysis

--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.

To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.

--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/MWHPR03MB281676B9A3440FA3FA7F050EA1BC0%40MWHPR03MB2816.namprd03.prod.outlook.com.

John Henning

unread,
Nov 15, 2016, 12:23:16 PM11/15/16
to material...@googlegroups.com

Your Code basis for that comment?  Opinions don’t matter – cite the Code basis.

 

From: material...@googlegroups.com [mailto:material...@googlegroups.com] On Behalf Of Shaunak Upadhyay
Sent: Monday, November 14, 2016 6:12 PM
To: material...@googlegroups.com
Subject: RE: [MW:25695] Tube to Tubesheet Joint

 

No. You cannot use 10.0mm PQR for tube to tubes heel joint.

On 15 Nov 2016 02:07, "John Henning" <jhen...@deltak.com> wrote:

Minor adjustment - ASME Section VIII Div. 1 does not mandate tube-to-tubesheet mockup for qualification  - however Division 2 does.

 

From: material...@googlegroups.com [mailto:material...@googlegroups.com] On Behalf Of George Dilintas
Sent: Sunday, November 13, 2016 7:28 AM
To: Meghanadh K
Subject: Re: [MW:25676] Tube to Tubesheet Joint

 

Taking into account that your Pno is 43 you may benefit of the provisions of  QW 202.4.

However before take a final decisions check the requirements of QW 202.6

2016-11-12 16:23 GMT+02:00 'prem_nautiyal26' via Materials & Welding <material...@googlegroups.com>:

Hi

 

Assuming your construction code is ASME SEC VIII div.1, 

You will have to carry out a separate tube to tube sheet mock up qualification.

Refer ASME SEC IX and SEC VIII Div 1 for details.

Also tube to Tube sheet mock up qualification will be mentioned in your approved QAP

 

 

 

REGARDS

 

 

PREM NAUTIYAL 

9769316004

 

 

 

 

 

 

Sent from my Samsung Galaxy smartphone.

-------- Original message --------

From: pankaj phuse <pankaj...@gmail.com>

Date: 11/11/2016 16:15 (GMT+05:30)

To: Materials & Welding <material...@googlegroups.com>

Subject: [MW:25662] Tube to Tubesheet Joint

 

Dear Experts,

 

Need your guidance on the following:

 

We have tube to tube-sheet joint having Groove + Fillet Weld without grooves & expansion. (Tube-2.7mm, Tubesheet-45mm, P No.43 to P. No.43)

 

I have PQR qualified on plate 10mm Thk. (P No.43 to P No.43, Qualification Range - 1.5 to 20mm).

 

Can I use the same WPS for this joint or we have to qualify new procedure.

 

Procedure qualified as per ASME Sec.IX.

 

Need clarification with reference to clause number.

 

--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.

To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To post to this group, send email to material...@googlegroups.com.

--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.

To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To post to this group, send email to material...@googlegroups.com.



 

--

Dr. Georgios Dilintas,

Dipl. Ing. In Aeronautic and Space Engineering

Ph.D in Mechanics of Solids - Computational Mechanics

A.I.S, A.N.I, IRCA Lead Auditor

Welding, Stress Analysis, Corrosion, QA/QC, Failure Analysis, Risk Analysis

--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.

To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To post to this group, send email to material...@googlegroups.com.

--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.

To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To post to this group, send email to material...@googlegroups.com.

--

http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.

To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To post to this group, send email to material...@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAD1AzTQzozVFNp05ThrFSEKD_0KLqwn-SAKgTLMhL7WsGrEXaQ%40mail.gmail.com.

Nitin Shetty

unread,
Nov 19, 2016, 7:06:01 AM11/19/16
to material...@googlegroups.com
Dear Pankaj,

ASME Sec VIII Div 1 does not require a mock up test to be performed. it is required only for Div 2. Coming back to your question whether you can use the existing PQR for tube to tube sheet welding-- My answer is yes you can use it. please check your client spec if they have asked for tube to tube sheet mockup as some clients do ask for it. Even if they ask or they don't ask for it you can very well use the existing PQR (Grove wed) for the tube to tube sheet welding. Hope your query is answered.

Regards,

Nitin Shetty

To: Materials & Welding <materials-welding@googlegroups.com>

Subject: [MW:25662] Tube to Tubesheet Joint

 

Dear Experts,

 

Need your guidance on the following:

 

We have tube to tube-sheet joint having Groove + Fillet Weld without grooves & expansion. (Tube-2.7mm, Tubesheet-45mm, P No.43 to P. No.43)

 

I have PQR qualified on plate 10mm Thk. (P No.43 to P No.43, Qualification Range - 1.5 to 20mm).

 

Can I use the same WPS for this joint or we have to qualify new procedure.

 

Procedure qualified as per ASME Sec.IX.

 

Need clarification with reference to clause number.

 

--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.

To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.

--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.

To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.



 

--

Dr. Georgios Dilintas,

Dipl. Ing. In Aeronautic and Space Engineering

Ph.D in Mechanics of Solids - Computational Mechanics

A.I.S, A.N.I, IRCA Lead Auditor

Welding, Stress Analysis, Corrosion, QA/QC, Failure Analysis, Risk Analysis

--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.

To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.

--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.

To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.

--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.

To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.

--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/MWHPR03MB2816AE26B8D89A5A90BAC9EDA1BF0%40MWHPR03MB2816.namprd03.prod.outlook.com.
Reply all
Reply to author
Forward
0 new messages