RE: 16910] Feasibility of repair welding for 4145h steel

551 views
Skip to first unread message

pgoswami

unread,
Mar 1, 2013, 11:15:34 PM3/1/13
to material...@googlegroups.com
Hi Ali,
 
These steels will have very high C.E. If you calculate as per the common IIW formula , the CE value would be > 0.55 or more. Generally weld repairs would not be advisable for drilling tools, due to safety and other serious damages to costly equipments. You may seek the opinion of the tool manufacturers and then decide.
 
Should weld repair be the  last resort, you may contact UTP (from my experience I've found them as a good resource for many "uncommon "  weld repair products).
 
Thanks.
 
 

Pradip Goswami,P.Eng.IWE

Welding & Metallurgical Specialist

Ontario, Canada.

Email-p...@sympatico.ca,

pgos...@quickclic.net



From: material...@googlegroups.com [mailto:material...@googlegroups.com] On Behalf Of Ali Momeni
Sent: Thursday, February 28, 2013 4:39 PM
To: material...@googlegroups.com
Subject: [MW:16910] Feasibility of repair welding for 4145h steel

All Dear
You know
"AISI 4145H is a chromium molybdenum quality alloy steel specification. As a high tensile steel grade AISI 4145H is primarily supplied in the hardened and tempered 
condition to 30-36HRc range to AISI 4145H modified. With a slightly higher carbon content AISI 4145H is similar to AISI 4140 in that it offers good ductility, shock  resisting characteristics combined with resistance to wear. and used in Well Drilling Tools"
and question is
"How can we evaluate the feasibility of repair welding for 4145H steel so that the properties needed to meet?"

--
To post to this group, send email to material...@googlegroups.com
To unsubscribe from this group, send email to materials-weld...@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
For more options, visit https://groups.google.com/groups/opt_out.
 
 
Outlook.jpg
drill_stem.pdf

khalid...@gmail.com

unread,
May 6, 2014, 5:34:27 AM5/6/14
to material...@googlegroups.com
Dear 
Could you please insist the electrode and filler for welding 316 to 4145H. 
Your earlier response in this regard is highly appreciated. 

On Sunday, March 3, 2013 1:40:38 AM UTC+5:30, Ali Momeni wrote:
Dear Pradip

Thanks for the your suggestions and answer.
But I must find a way to repair them, and I think the control of welding parameters and heat treatment, can be achieved me to the optimal properties.
 

khalid...@gmail.com

unread,
May 9, 2014, 2:15:06 AM5/9/14
to material...@googlegroups.com
Dear Members
Could you please insist the electrode and filler for welding material grade 316 to 4145H and the parameters details.
What will be the P & G number for API7-1 Gr.4145H  
Your earlier response in this regard is highly appreciated.

Thanking You
--
Regards
Khalid Mulla

Harish Kannepalli

unread,
May 9, 2014, 7:48:25 AM5/9/14
to material...@googlegroups.com
Mr. Ali,
            Please look matching chemistry and mechanical properties in the electrode. These type of materials are not listed in any code. You have to develop your own procedure. Contact any electrode manufacturer for nearest matching electrode and welding parameters.


2013-03-01 1:39 GMT+04:00 Ali Momeni <azandar...@gmail.com>:
All Dear
You know
"AISI 4145H is a chromium molybdenum quality alloy steel specification. As a high tensile steel grade AISI 4145H is primarily supplied in the hardened and tempered 
condition to 30-36HRc range to AISI 4145H modified. With a slightly higher carbon content AISI 4145H is similar to AISI 4140 in that it offers good ductility, shock  resisting characteristics combined with resistance to wear. and used in Well Drilling Tools"
and question is
"How can we evaluate the feasibility of repair welding for 4145H steel so that the properties needed to meet?"

--
To post to this group, send email to material...@googlegroups.com
To unsubscribe from this group, send email to materials-weld...@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
For more options, visit https://groups.google.com/groups/opt_out.
 
 



--
regards,
Harish.