Following is example to explain the conditions
Condition 1
As per manufacturer (Say manufacturer ABC) the Flux and Wire combination mentioned on the data sheet and bag of flux is F7A8-EH12K and is inline with the ASME Sec II Part C SFA 5.17
Where “A” is as welded condition
PQR was qualified with PWHT using above mentioned manufacturers flux wire combination.
Question
1. Can I write on my PQR and WPS write the Flux wire classification as F7P8-EH12K
2. Batch of flux and wire used in PQR shall only be used in Production welding.
Condition 2
I use a Flux from manufacturer ABC and wire from manufacturer XYZ. Manufacturer ABC who is the manufacturer of Flux has certified the flux on bag as F7A8-EH12K (when I say this, I mean the manufacturer ABC has used both flux and wire from manufacturer ABC)
My actual conditions are I am using different manufactures for flux and wire to qualify PQR
PQR was qualified with PWHT
Question
1. Can I use different manufacturer for flux and wire
2. Can I write on my PQR and WPS write the Flux wire classification as F7P8-EH12K
3. Batch of flux and wire used in PQR shall only be used in Production welding.
Appreciate your advice for me to understand and if any reference document which I can review of the subject to clarify.
--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To view this discussion visit https://groups.google.com/d/msgid/materials-welding/0f907ff4-734e-4084-8059-127bb4b37b5dn%40googlegroups.com.
Thanks & Regards
J.Gerald Jayakumar
0091-8838619635
Following is example to explain the conditions
Condition 1
As per manufacturer (Say manufacturer ABC) the Flux and Wire combination mentioned on the data sheet and bag of flux is F7A8-EH12K and is inline with the ASME Sec II Part C SFA 5.17
Where “A” is as welded condition
PQR was qualified with PWHT using above mentioned manufacturers flux wire combination.
Question


2. Batch of flux and wire used in PQR shall only be used in Production welding. - NO RESTRICTION in Code
Condition 2
I use a Flux from manufacturer ABC and wire from manufacturer XYZ. Manufacturer ABC who is the manufacturer of Flux has certified the flux on bag as F7A8-EH12K (when I say this, I mean the manufacturer ABC has used both flux and wire from manufacturer ABC)
My actual conditions are I am using different manufactures for flux and wire to qualify PQR
PQR was qualified with PWHT
Question
2. Can I write on my PQR and WPS write the Flux wire classification as F7P8-EH12K - NO
3. Batch of flux and wire used in PQR shall only be used in Production welding. _ NO
Appreciate your advice for me to understand and if any reference document which I can review of the subject to clarify.