Dear Experts

What is the Radiography requirement for category D fluids with
reference to B31.3

Regards
--
maran

CHINTUKUMAR GANDHI

unread,
Mar 30, 2014, 8:22:04 AM3/30/14
to material...@googlegroups.com
Dear Mr. Maran,

With reference to the clause no. 341.4.2 of ASME B31.3 only visual Exam. is required. Please refer Para 341.3.2 for accept. criteria.

Thanks & regards,


C. R. GANDHI


From: Elamaran Rajan <elams...@gmail.com>
To: materials-welding <material...@googlegroups.com>
Sent: Friday, March 28, 2014 5:57 PM
Subject: [MW:20425] RT requirement for cat D fluids
--
To post to this group, send email to material...@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsub...@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm

The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsub...@googlegroups.com.
For more options, visit https://groups.google.com/d/optout.


Shashank Vagal

unread,
Apr 2, 2014, 1:35:43 AM4/2/14
to material...@googlegroups.com
Gents,
·                     Category D:
Flammable, unstable or toxic fluids which are gases or a mixture of gas and liquid with a TGLR>250 but H2S < 500 ppm in the gas phase at prevailing ambient temperature and atmospheric pressure plus 0.5 bar, i.e. the vapour pressure is higher than 1.5 bar (abs) at ambient temperature. Example: natural gas, liquid petroleum gas, ammonia, typical’ low risk sour facility’ or high GOR oil condensate and gas flowline fluids.
Extent of Required Examination:
"Examination" is not limited to welds. Records, materials, fabrication, erection pressure testing, as-built, must also be examined as specified by Code. Refer to Table 3 of 341.4.2 of ASME B31.3, for a list of examination attributes and the extent of required examination.

Table 3 - EXAMINATION OF MATERIALS, FABRICATION AND INSTALLATION
Extent of Required Examination
Material
Fabrication
Fabrication of Longitudinal Welds
Mechanical Joints
Erection
Complete system Meets Design (2)
Other Examinations
Category D
Random
Random
Random
Random
Random
Random
Random (3)
Normal
Random
5%(5)
100%
Random(1)
Random
Random
5% Vol. (4)
Category M
Random
100%
100%
100%
Random
Random
20% Vol.
High Pressure
100%
100%
100%
100%
Random
Random
100% Rad.
Severe Cyclic
Random
100%
100%
100%
100%
Random
100% Vol.
Notes: (1) When pneumatic testing is to be used, 100% of mechanical joints shall be examined. (2) Includes any additional examination or testing required by engineering. (3) Category D Systems require welds to be random visually examined.
(4) When brazed joints are used, 5% in-process examination is performed. (5) Socket welds require 5% visual examination of final weld. Note: Vol = Volumetric weld examination such as a radiography or ultrasonic. Rad = Radiography
 
With Best Regards,
To unsubscribe from this group, send email to materials-weld...@googlegroups.com

For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.

sid

unread,
Mar 9, 2020, 4:15:45 AM3/9/20
to Materials & Welding
Dear all,

Need answer of this below question please help out with correct answer.

*Extent of radiography for catagory D fluid? 


Regards
Sid

atul khatri

unread,
Mar 9, 2020, 11:19:44 AM3/9/20
to material...@googlegroups.com
Hi ,

Radiography is not required for category "D" fluid as per ASME B 31.3.

Best Regards
Atul Khatri


---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.

Prasanta Kumar Pal

unread,
Mar 9, 2020, 11:19:44 AM3/9/20
to material...@googlegroups.com
RT does not depend upon only category of fluid. See the other criteria.

--

Davis Boyer

unread,
Mar 9, 2020, 11:19:44 AM3/9/20
to material...@googlegroups.com
Believe inspection is option of category D fluids per 31.3

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/eaff11fd-d447-4129-8feb-a71fc295999c%40googlegroups.com.
--
Davis Boyer
Player Advisor - Top Shelf Sports Management

Charles Jacob

unread,
Mar 9, 2020, 11:19:44 AM3/9/20
to material...@googlegroups.com
Dear, 

RT required is 1 in 20 

Regards, 

Charles V Jacob 

--

james gerald

unread,
Mar 9, 2020, 11:19:45 AM3/9/20
to material...@googlegroups.com
Only Visual examination and no RT requirement.


Inline image

Thanks & Regards

J.Gerald Jayakumar



Kannayeram Gnanapandithan

unread,
Mar 10, 2020, 11:30:25 PM3/10/20
to materials-welding
Ref B 31.3-2018,  341.4.2. Examination- Category D Fluid

Reply all
Reply to author
Forward
0 new messages