SM490A weld to railway

134 views
Skip to first unread message

Pravin Poornachandran

unread,
Apr 8, 2021, 6:51:12 AM4/8/21
to 'Bijay' via Materials & Welding
Dear Expert,

We are doing a weld joint with following base metal combination: 
SM490 weld to railway (alloyed, high tensile material) 

I used E7016 for this welding, after 4 hours, crack was observed on the weld toe,
however there is no crack on the weldment, thus I assume this is cold crack. 

Crack was noticed on the railway material, not on SM490A material. 

Welding condition:
Baking was done 300-350degC x 1hr 
thickness: 16mm both material 
Preheat: 200degC 
Post heating: 250degC x 1hr

Can anyone advise how to solve this crack defects

Best regards,
Pravin Poornachandran

Vishwas Keskar

unread,
Apr 8, 2021, 8:04:22 AM4/8/21
to material...@googlegroups.com
Pl. send MTCs of both the materials 

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CADDyn7eE6%2Ba9MxkOJQ6oTfKK3xFXmLvXGn0yp5cFjAzWpGt_-A%40mail.gmail.com.

Pravin Poornachandran

unread,
Apr 10, 2021, 12:16:15 AM4/10/21
to material...@googlegroups.com

Dear Sir,

 

Enclosed material properties of railway material, while SM490A is ordinary mild steel with low carbon content <0.3%

Along I have enclosed picture of the crack.

 

1st picture was without preheat, while 2nd picture was with preheat 230degC & postheating 250degC x1hr.

However, crack still occurs. I’m bit lost at this point.

 

Sent from Mail for Windows 10

Gantrail_Enclosed_Arc_Crane_Rail_Welding_Datasheet (5).pdf
JIS-37-A-KG.pdf
WhatsApp Image 2021-04-08 at 09.04.47.jpeg
WhatsApp Image 2021-04-08 at 16.13.14.jpeg

Vishwas Keskar

unread,
Apr 10, 2021, 12:40:39 AM4/10/21
to material...@googlegroups.com
Railway material is  with High Carbon  so will have  high strength  with  High HAZ hardness .

The electrode deployed - E7016 has less strength .

Use E11018   with pre heating   and 3.15  dia with stringer bead technique.
After full welding , maintain pre ehat maintenance  say 350  Deg C - 2 HRS  and then cool under insulation 

This shall 

pravin.n...@gmail.com

unread,
Apr 10, 2021, 8:33:48 AM4/10/21
to Materials & Welding
E-7016 not be suitable for SM490A to Rail steel (low alloy steel)

Below suggestion given based on both material Chemical & Mechanical properties.
Sugeested welding consumable for SM490A to Rail steel (low alloy steel) is E-12016-G electrode
Preheat temp. for the rail steel- 200 to 300 Deg.C
Interpass Temp.:- Less than 400 Deg.C
Slow cooling required after welding by insulation covering.

Regards,
Pravin Nimbalkar
Welding Engineer

Satyaprakash Soni/EM&RBG/MUM

unread,
Apr 10, 2021, 8:33:49 AM4/10/21
to material...@googlegroups.com
avoid faster colling rate.

Thanks & Regards,
Satyaprakash Soni,Manager - QA/QC,Mobile +91-9892649099



****---------------------------**** 
Disclaimer : The information contained in this e-mail (including any attachments) is privileged and confidential. If you have received it by mistake please notify the sender by return e-mail and permanently delete this e-mail and any attachments from your system. Any dissemination, use, review, distribution, printing or copying of this message in whole or in part is strictly prohibited. Please note that e-mails are susceptible to change. Voltas Ltd. (including its group companies) shall not be liable for the improper or incomplete transmission of the information contained in this communication nor for any delay in its receipt or damage to your system. Voltas Ltd. (or its group companies) does not guarantee that the integrity of this communication has been maintained or that this communication is free of viruses, interceptions or interference.

Ramin Kondori

unread,
Apr 10, 2021, 11:05:59 AM4/10/21
to material...@googlegroups.com
Is this the new Japanese high-speed rail project in India...?

Ramin  Kondori
Sr. QA/QC & Welding Engineer
-----------------------------------------------------------
PG-Dip. in Welding Engineering (IWE  AT  0070)
BSc. in Civil Engineering (IUT)
BGAS Painting Inspector
ASNT Level I&II
                        
IIW-Logo-Colour-small


--

Pravin Poornachandran

unread,
Apr 11, 2021, 10:52:09 AM4/11/21
to material...@googlegroups.com

Hi Ramin,

 

This is in Malaysia high speed rail project which connects North – East Malaysia.

 

Sent from Mail for Windows 10

 

From: Ramin Kondori
Sent: Saturday, 10 April, 2021 11:05 PM
To: material...@googlegroups.com

Pravin Poornachandran

unread,
Apr 11, 2021, 10:52:09 AM4/11/21
to material...@googlegroups.com

Hi Pravin,

 

Thank you very much for your valuable inputs.

I shall take note.

 

Sent from Mail for Windows 10

 

Pravin Poornachandran

unread,
Apr 11, 2021, 10:52:09 AM4/11/21
to material...@googlegroups.com

Hi Vishwas,

 

I agree with you on the electrode selection.

Need your advice, using high tensile electrode can lead to brittleness?

The problem im facing now is, client keep on insisting to use E7016 instead of high tensile electrode.

 

Having hard time to convince the client.

 

Anyways appreciate your input.

Vishwas Keskar

unread,
Apr 12, 2021, 12:55:48 AM4/12/21
to material...@googlegroups.com
Dear Pravin,

Query- 
Need your advice, using high tensile electrode can lead to brittleness?
Response - 
These High Tensile electrodes are with Low alloys addition and have moderate ductility of @20 %-  reasonable ductility during Welding 
Need  to follow  critical Welding parameters  , the welding will be sound .
 
Query-
The problem im facing now is, client keep on insisting to use E7016 instead of high tensile electrode.
  Response - The rail material is High Carbon  so hard HAZ requires strength when  butt  Joint is welded.  So either E110XX, E120XX is chosen
For Fillet welds , E7016 would have been suffice 

Hope the things will  be all clear


  

Reply all