regarding- thickness range for LTCS piping material for WPS

1,031 views
Skip to first unread message

Darshan Maheshwari

unread,
Apr 19, 2012, 1:42:35 AM4/19/12
to material...@googlegroups.com
Can any body suggest what thickness range is applied for qualifying a WPS (for thickness 7.11mm) for LTCS piping material. Please provide reference also.
 
Regards,

Darshan Maheshwari.

Raghuram Bathula

unread,
Apr 19, 2012, 4:09:53 AM4/19/12
to Materials & Welding
what is your design code?
As per ASME it will be T-2T, however for piping (B31.3) this range can
be used if PTC's are provided for the thickness ranges as specified in
Table 323.3.1, else it will be T to T+6mm

Best regards

On Apr 19, 10:42 am, Darshan Maheshwari <darshan.maheshw...@yahoo.com>
wrote:

Karthik

unread,
Apr 19, 2012, 4:15:50 AM4/19/12
to material...@googlegroups.com
As per ASME Sec.IX QW451.1 thickness of test coupon is 1.5mm to mm means the thickness qualified limit is 1.5mm (Minimum) and 2T(Maximum).
In your case, If you use 7.11mm thickness specimen for PQR then the Thickness Qualified limit will be 1.5mm to 14.22mm.
 
Thanks & Regards,

(Karthik)

Karthikeyan.S
QA/QC Manager
German-Thai Boiler Engineering Cooperation Limited.
Rayong Factory ;
379 Moo.6 Soi 8, Tambol Pananikom,
Nikompattana, Rayong 21180 THAILAND
Tel : +66 38 897 035-9 Ext. 137
Hand Phone: 0066 892512282


From: Raghuram Bathula <raghura...@gmail.com>
To: Materials & Welding <material...@googlegroups.com>
Sent: Thursday, April 19, 2012 3:09 PM
Subject: [MW:14128] Re: regarding- thickness range for LTCS piping material for WPS
--
To post to this group, send email to material...@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsub...@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.


CHINTUKUMAR GANDHI

unread,
Apr 21, 2012, 8:12:52 AM4/21/12
to material...@googlegroups.com
Dear Mr. Darshan,
 
As per QW-403.6 & QW-403.8 of ASME Sec. IX, if PQR will be done on 6 mm. thk. P -1, G-1 material, your qualified base metal thk. range shall be minimum 6 mm. to max. 12 mm. Kindly check for PWHT- Normalizing. 
 
Thanks & regards,
 
 
C. R. GANDHI

--- On Thu, 4/19/12, Darshan Maheshwari <darshan.m...@yahoo.com> wrote:
--
To post to this group, send email to material...@googlegroups.com
To unsubscribe from this group, send email to materials-weld...@googlegroups.com

sreedhar ch

unread,
Apr 22, 2012, 1:00:49 AM4/22/12
to material...@googlegroups.com
ASME Sec IX(QW 403.6) 7.11mm to 14.22mm, With Impact testing.
Minimum Thickness of Base metal qualified is the thickness of test coupon or 16 mm which ever is minimum.
 
Sreedhar

--

PRAMODH NAIR

unread,
Apr 24, 2012, 7:50:37 AM4/24/12
to material...@googlegroups.com
If the consturction code is B31.3, the LTCS materail qualified range is 1/2T to T+6mm.
 
Pramodh

Don Under Survilliance

unread,
Apr 26, 2012, 3:49:44 AM4/26/12
to material...@googlegroups.com
hello darshan
its Ajay here
 
your thickness limit will be 7.11 to 14.22
this is as per ASME sec IX......bcouse for LTCS u have to do the impact test............in dis case ur limit will me in lower side is 7.11 but limited to 2T in higher side........
jus go thorugh ASME sec IX chapter 4 clause no QW-403.6

QW-403.6

The minimum base metal thickness qualified

is the thickness of the test coupon

T or 58 in. (16 mm),

whichever is less. However, where

T is less than 14 in.

(6 mm), the minimum thickness qualified is

12T. This variable

does not apply when a WPS is qualified with a PWHT

above the upper transformation temperature or when an

austenitic or P-No. 10H material is solution annealed after

welding.



On Thu, Apr 19, 2012 at 11:12 AM, Darshan Maheshwari <darshan.m...@yahoo.com> wrote:

--

Karunakaran Karan

unread,
Aug 23, 2015, 9:13:53 AM8/23/15
to Materials & Welding, darshan.m...@yahoo.com

Dears,
         Good day.I have one doubt about LTCS PQR regarding
temperature limit.Our PQR specimen is 5mm thickness and impact test at
2.5mm thick.In your design
temp.is -46 degree.In ASME 31.3 and section
viii says .this 2.5 mm specimen allowed for -27degree.But our client comment is this PQR IS used only
-28 degree only.So explain about the correct thickness of specimen for
impact test at -46 temp.design temp.

Thanks and Regards