I have query regarding hardness testing in pipe weld size 2" to 30".
Have any procedure or code for taking nos of reading for hardness.
Like 2"-to 6"
8"- to 14"
16"- to 30".

Regards

Lalit Vadadoriya
Dy.Manager(Piping)
Engineers India Limited

Raghuram Bathula

unread,
Aug 21, 2019, 5:35:47 AM8/21/19
to Materials-Welding
None, refer NACE RP 472 for guidelines
Generally average of 3 readings , and some client spec states 120 ° apart etc..
-- 

LALIT VADADORIYA

unread,
Jul 18, 2024, 11:39:12 PM7/18/24
to material...@googlegroups.com


Dear Group members,

I have query regarding hardness testing in pipe weld size 2" to 30".
Have any procedure or code standards for taking nos of reading for hardness test on Pipe weld like diff sizes..
Like 2"-to 6"
8"- to 14"
16"- to 30".

Regards

Lalit Vadadoriya
Engineers India Limited

kingslygeo vargheese

unread,
Jul 20, 2024, 2:56:32 AM7/20/24
to material...@googlegroups.com
Dear Lalit,

Based on client specification

Hardness tests on a production weld shall include a reading on the centre of the weld and the heat affected zones on both sides of the weld. The hardness test of the heart affected
zone shall be made at a point as near to the edge of the weld as practicable.

Each test area three impacts shall be carried out and the average of these shall be recorded. All results and averages shall be recorded on the Hardness Test InspectionReport.

Butt welds on pipes of nominal size upto and including DN100 (4") one set of
readings shall be taken on the 12 o' clock position or 6 o' clock position

Butt welds on pipes of nominal size from DN150 (6”) to DN300 (12”), two sets of
readings shall be taken 120° apart, with one set on the 12 o' clock position & o' clock
position

Branch connections and fillet welds on pipes of all diameters, two sets of
readings 180° apart shall be taken.

Note: location shall be approved by CONTRACTOR/COMPANY prior inspection

Best Regards
V.Kingsly Geo.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAKjb_1KVOXu-E7VC3EYJxVmsucb9J%3D04peESYX5eqMv-b%3DhiFw%40mail.gmail.com.

Faisal Quadri

unread,
Jul 20, 2024, 3:18:11 AM7/20/24
to material...@googlegroups.com
what is your project, construction code, check first your project specifications, we can not generalize, different standard different requirements ?

 


FAISAL QUADRI

3736 Salman Al Farisi King Abdul Aziz Sea Port
Unit No.1 Dammam 32213-7911, K.S.A

Mobile: +966 53 7253477

Email: f.qu...@amo.com.sa | Web: www.amo.com.sa



--
Reply all
Reply to author
Forward
0 new messages