Is P11 to Satainless Steel(304L or 316L) welding possible?

1,796 views
Skip to first unread message

Ganesh Mahankal

unread,
Mar 19, 2014, 9:05:37 AM3/19/14
to material...@googlegroups.com
 
Dear All ,
 
Is P11 to Stainless Steel(304L or 316L) welding possible?
 
If yes then plz mention by which welding consumables?
 
Best Regards,
 
Ganesh Mahankal
Alfa Laval India Ltd.Pune India
 

george....@gr.bureauveritas.com

unread,
Mar 20, 2014, 6:24:40 AM3/20/14
to material...@googlegroups.com

Yes,
 you may use 309 grade, in order to avoid hot cracking because of low FN.
 If your P11 pipe has to undergo PWHT because of thickness, then you have to butter the P11 with 309, perform the PWHT and then weld it to the 316 using again the 309 filler metal.
This will help you to avoid sensitization of 316.
 However, the buttered area has to undergo a corrosion test if the pipe is for wet service and clorines may be present.
For buttering you may need a specific WPS qualification (see ASME IX QW-283)

    best regards

    Dr. Georgios Dilintas

    Authorized Nuclear Inspector
    Authorized Inspector Supervisor
    API 510 Inspector

    I&F REGIONAL TECHNICAL MANAGER
    BUREAU VERITAS HELLAS

    Tel: +30 210 40 63 113/4
    Fax: +30 210 40 63 118
    Cell: +30 69 44 64 62 04
    (See attached file: Dilintas_George.vcf)

Inactive hide details for Ganesh Mahankal ---20/03/2014 00:57:47---  Dear All ,Ganesh Mahankal ---20/03/2014 00:57:47---  Dear All ,

--
To post to this group, send email to material...@googlegroups.com
To unsubscribe from this group, send email to materials-weld...@googlegroups.com
For more options, visit this group's bolg at
http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm

The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to
materials-weld...@googlegroups.com.
For more options, visit
https://groups.google.com/d/optout.

This message contains confidential information. To know more, please click on the following link: http://disclaimer.bureauveritas.com

Dilintas_George.vcf

kannayeram gnanapandithan

unread,
Mar 20, 2014, 7:17:02 AM3/20/14
to materials-welding
use E NiCrFe3 /ER NiCr3

THANKS & BEST REGARDS
KG.PANDITHAN, AWS-CWI, CSWIP 3.1
CONSULTANT-WELDING & QUALITY

Azam Mohd

unread,
Mar 20, 2014, 6:11:35 AM3/20/14
to material...@googlegroups.com

Use below filler wire and electrode, Having good weldability. We have qualified PQR with this consumable:

ERNiCr-3/ ENiCrFe-3




--

deejos...@gmail.com

unread,
Sep 28, 2021, 11:15:37 PM9/28/21
to Materials & Welding
Can anyone share WPS for P11-335 to SS321 OR SS316

Vishwas Keskar Welding Manager WELDING

unread,
Sep 29, 2021, 3:51:12 AM9/29/21
to Materials & Welding
Dear Ganesh 

The compatible filler metal shall be decided based on 
1) Service temperature 
2) Type of butt joint - Butt/ fillet 
3) PWHT required or not 
4)Service type -Elevated/corrosion  etc

Pl. state all the requirements from drawing/specs   then we experts can give suitable advice 

Vishwas 
9823472273 
Head - Welding Technology

José Juan Jiménez Alejandro

unread,
Oct 1, 2021, 4:36:57 AM10/1/21
to material...@googlegroups.com


---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
Reply all
Reply to author
Forward
0 new messages