Corrosion Test Fail For Duplex Steel

266 views
Skip to first unread message

Ashish Chacko

unread,
Jul 18, 2023, 1:26:20 AM7/18/23
to Materials & Welding

I am currently working on developing a Procedure Qualification Record (PQR) for Duplex Steel. In the process, I conducted welding using the base material SA 790 (UNS:32205) and utilized two different filler wires: ER-2594 and ER-Nicr-Mo-14 for different coupons. Size of the coupon 6" Thick:10.97 mm.

However, I encountered a concern during the corrosion testing phase, as per ASTM A923-03 standards. Both test materials failed the corrosion test. I'm seeking guidance from the experts in this group to understand the possible reasons for the failure and to explore potential solutions or alternative approaches.

If anyone has experience with similar issues or insights into the matter, I would greatly appreciate your assistance.

Vishwas Keskar

unread,
Jul 18, 2023, 4:10:50 AM7/18/23
to material...@googlegroups.com
What was the backing and shielding gas ?

Sent from my iPhone

On 18-Jul-2023, at 10:56 AM, Ashish Chacko <iamash...@gmail.com> wrote:



I am currently working on developing a Procedure Qualification Record (PQR) for Duplex Steel. In the process, I conducted welding using the base material SA 790 (UNS:32205) and utilized two different filler wires: ER-2594 and ER-Nicr-Mo-14 for different coupons. Size of the coupon 6" Thick:10.97 mm.

However, I encountered a concern during the corrosion testing phase, as per ASTM A923-03 standards. Both test materials failed the corrosion test. I'm seeking guidance from the experts in this group to understand the possible reasons for the failure and to explore potential solutions or alternative approaches.

If anyone has experience with similar issues or insights into the matter, I would greatly appreciate your assistance.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/8de07ffa-c770-4e90-ab75-f83b3089d3b0n%40googlegroups.com.

Vishwas Keskar

unread,
Jul 18, 2023, 4:10:50 AM7/18/23
to material...@googlegroups.com
Pl share the test results 


Sent from my iPhone

On 18-Jul-2023, at 10:56 AM, Ashish Chacko <iamash...@gmail.com> wrote:



I am currently working on developing a Procedure Qualification Record (PQR) for Duplex Steel. In the process, I conducted welding using the base material SA 790 (UNS:32205) and utilized two different filler wires: ER-2594 and ER-Nicr-Mo-14 for different coupons. Size of the coupon 6" Thick:10.97 mm.

However, I encountered a concern during the corrosion testing phase, as per ASTM A923-03 standards. Both test materials failed the corrosion test. I'm seeking guidance from the experts in this group to understand the possible reasons for the failure and to explore potential solutions or alternative approaches.

If anyone has experience with similar issues or insights into the matter, I would greatly appreciate your assistance.

--

Ashish Chacko

unread,
Jul 18, 2023, 7:16:47 AM7/18/23
to Materials & Welding
Backimh and shieldimg gas was argon grade 4.7 b ( 99.997%)

james gerald

unread,
Jul 18, 2023, 7:16:47 AM7/18/23
to material...@googlegroups.com
1. The suitable welding consumable for welding SA 790 (UNS32205) is ER2209.
2. To pass ASTM G48 test, some  prefer using ER 2594  for the root pass (though it is a super Duplex SS).
3. The formation of Intermetallic compounds as detected IN ASTM A923 is because of below reasons.

    a.  Use of higher Alloy content consumable.
    b.  High Heat Input which in turn  reduces the cooling rate and inturn increase the time spent in the higher         
         temperature region which results in forming Intermettalic phases like Sigma phase and Chi phase.

Please provide a copy of WPS to understand the welding conditions. 

Also provide ASTM A923 Test Report.

Thanks & Regards

J.Gerald Jayakumar



--

Ashish Chacko

unread,
Jul 18, 2023, 7:16:47 AM7/18/23
to Materials & Welding
Dear Kindly find the test report

On Tuesday, 18 July 2023 at 11:10:50 UTC+3 Vishwas Keskar wrote:
SKM_C30823071715530.pdf

Ahmad el-sharkawy

unread,
Jul 18, 2023, 7:16:48 AM7/18/23
to material...@googlegroups.com
Please share with us the corrosion report and photos for corrosion testing as well, porposed WPS and PQR as run sheet.

Babur Khan

unread,
Jul 18, 2023, 11:38:44 PM7/18/23
to material...@googlegroups.com
Greetings,
In pas we faces same issue and after that we get recommendations from test laboratories to use mixture gases for shielding and purging.
Argon + 2% Nitrogen mixer with ER2594 filler wire.a

 Babur Khan Lashari 

Sent from my iPhone

On 18 Jul 2023, at 2:16 PM, Ashish Chacko <iamash...@gmail.com> wrote:

Backimh and shieldimg gas was argon grade 4.7 b ( 99.997%)

G Neethipathi

unread,
Jul 18, 2023, 11:48:40 PM7/18/23
to material...@googlegroups.com
Better try with ER347 Filler wire.for duplex steel this filler material is suitable.

T/R

--

Pham Thanh Tinh

unread,
Jul 19, 2023, 1:03:57 AM7/19/23
to material...@googlegroups.com
Hi 

Send to me all PQT report from your conduct I will support to you.

Vào Th 3, 18 thg 7, 2023 vào lúc 08:26 Ashish Chacko <iamash...@gmail.com> đã viết:

I am currently working on developing a Procedure Qualification Record (PQR) for Duplex Steel. In the process, I conducted welding using the base material SA 790 (UNS:32205) and utilized two different filler wires: ER-2594 and ER-Nicr-Mo-14 for different coupons. Size of the coupon 6" Thick:10.97 mm.

However, I encountered a concern during the corrosion testing phase, as per ASTM A923-03 standards. Both test materials failed the corrosion test. I'm seeking guidance from the experts in this group to understand the possible reasons for the failure and to explore potential solutions or alternative approaches.

If anyone has experience with similar issues or insights into the matter, I would greatly appreciate your assistance.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/8de07ffa-c770-4e90-ab75-f83b3089d3b0n%40googlegroups.com.


--
Best & Regard
Pham Thanh Tinh
QC Manager
China National Chemical Engineering Third Co.LTD
South Ghawar Gas Separation Plant & Associated Facilities Project
Mobile phone +966. 556802308 


Ashish Chacko

unread,
Jul 19, 2023, 1:10:13 AM7/19/23
to Materials & Welding
Kindly find the attachment for test report
SKM_C30823071715530.pdf

Aneesh

unread,
Jul 19, 2023, 1:55:41 AM7/19/23
to Materials & Welding
HI Ashish Chacko

You may use 87% Argon + 10%Helium +3% Nitrogen. (as backing and shielding)
Maintain inter pass temperature below 100 C. 
Use ER2594 Filler Wire (ESAB or DAIKO Brand)
Most importantly, make sure you do pickling and passivation after welding, for the time specified for Super duplex materials. ( you will find the time in 
pickling and passivation gel itself. We used S weld gel)

Im sure you will reap the result. we got Corrosion value as = 0 MDD

Thanks and Regards

Aneesh Kizhakkekalam
QA/QC Manager (Saudi Aramco Project)

Thanh Tĩnh Pham

unread,
Jul 19, 2023, 1:55:41 AM7/19/23
to material...@googlegroups.com
Share to me all run sheet records 

Sent from my iPhone

On 19 Jul 2023, at 08:10, Ashish Chacko <iamash...@gmail.com> wrote:

Kindly find the attachment for test report

james gerald

unread,
Jul 19, 2023, 10:50:54 PM7/19/23
to material...@googlegroups.com
Just to add a portion from API RP582.

Inline image


Thanks & Regards

J.Gerald Jayakumar


james gerald

unread,
Jul 19, 2023, 10:50:54 PM7/19/23
to material...@googlegroups.com
Gentlemen excuse me if I have interrupted. This is a  Forum where everybody shares their  Technical knowledge and experience so that it is useful to the concerned. Sometimes we may be wrong also and take it sportively without being offended.

Argon + 2% N2 mixture is highly recommended for purging and shielding for the below purposes.

1.  Nitrogen is an Austenite stabilizer and promotes Austenite formation in the duplex matrix.
2. It improves Pitting corrosion resistance.
3. The maximum solubility of Nitrogen in DSS A32205 is 0.2% and anything more than that will come out of the solution.
4. Nitrogen delays the formation of Intermetallic phases.
 Inline image
5. Nitrogen may be more efficient in aiding ASTM G48 corrosion test.


But in ASTM A923, the weight loss is mainly due to Intermetallic Phases as higher PREN electrodes used such as Super duplex and Nickel base electrodes does not cause in weight loss due to pitting corrosion. I feel the main reason is higher alloy contents of Cr, Mo,W in the welding consumable which causes Intermetallic phases. Though N2 mixture has some effect but unless care is taken on correct welding consumable it is difficult to prevent and also equally dependent on WElding conditions like Heat Input, Preheat and Interpass temperature.

Some portions below on sigma phase.

Inline image


Thanks & Regards

J.Gerald Jayakumar


On Wednesday, 19 July, 2023 at 09:08:39 am IST, Babur Khan <mbabu...@gmail.com> wrote:


J Prinsen

unread,
Jul 20, 2023, 4:00:04 AM7/20/23
to materials-welding
Gents,

In the past a had a project with Super-Duplex with the same problem.
To solve this we liked to use Ar-N2 as a backing gas, but this was not in stock.
We switched to 100% N2 as a backing gas, and this worked out well for the corrosion test (40 degrees centigrade for Super DSS) and the complete PQR
In all cases the use of cold pass technique (thicker root pass (HI 1.2 kJ/mm max, thin second pass) interpass max 150 centigrade, overall HI max 1 kJ/mm has to be maintained 

Regards

Ir. Jurgen Prinsen IWE
Metallurgical and Welding Engineer





Van: "materials-welding" <material...@googlegroups.com>
Aan: "materials-welding" <material...@googlegroups.com>
Verzonden: Woensdag 19 juli 2023 15:36:34
Onderwerp: Re: [MW:34431] Corrosion Test Fail For Duplex Steel