Happy Sunday to all. 

  A  48 " tubular having 25 mm thickness we made a single bevel butt joint. 

The root & Hotpass  is welded with GTAW and fill up and capping is welded with SMAW. 
My query is that, 

Is back welding  is required or not . If required , please tell the procedure of back welding.
I mean to ask ,
1. which welding process should I use GTAW or SMAW for back welding. ? 
2 . With back gouging or without  back gouging. ? 

Hany Nabil

unread,
Jul 10, 2022, 4:27:27 AM7/10/22
to material...@googlegroups.com
Depends on approved WPS 
Your WPS mentioned or not for back gouging ?

Thanks 

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CANDtUcF-8SZ%2BFOoa-TAaFqRO67EKXWL0bB-sjAb_SzhAuMRTpQ%40mail.gmail.com.
--


 Best Regards,

 Eng. Hany Nabil
 Senior QA / QC Welding Engineer
 Egypt Mobile: 002-01225622022


This message, including any attachments, may contain confidential and privileged information for the sole use of the intended recipient(s). Review, use, distribution or disclosure by others is strictly prohibited. If you are not the intended recipient, or authorised to receive information on behalf of the recipient, please contact the sender by reply email, and delete all copies of this message. While we have taken reasonable precautions to ensure that this message and any attachments are free from viruses, we cannot guarantee that they are virus free and accept no liability for any damage caused by this message or any attachments. Messages sent or received through our networks may be monitored to ensure compliance with the law, regulation and/or our policies.

srinivas rao

unread,
Jul 10, 2022, 4:27:49 AM7/10/22
to Materials & Welding

Hi Mahesh, 

if you want to go with double side welding it is allowed to do in many codes, however u need check in client specifications, are they allowing this or not, some client specification says change in sequence of qualified /approved welding procedure is not acceptable. 

 

if you want to weld this 48" x 25mm thickness both side welding, it is better to use full SMAW process to complete the joint faster.

u need to prepare a separate SMAW -WPS by using same PQR showing the joint configuration and take approval from client and proceed with welding, no client will object this.

back welding with GTAW may not preferable, it is allowed to do with GTAW also but it is not economical.

 

u can use GTAW for back welding by demonstrating the process though qualified PQR as welding parameters will be different from the earlier PQR qualified for back welding.


Thanks & Regards, 
Rao 

Lakshman Kumar

unread,
Jul 10, 2022, 4:27:56 AM7/10/22
to material...@googlegroups.com
Hi

For the inside welding requirements What is the specification or client requirements, weld joint efficiency considered during design, working pressure to design pressure (factor of safety) etc parameters will decide. 

If inside complete penetration, complete edges fusion happened no need to go for the inside seal run or capping else you can plan for the defect removal and can do the welding 

Coming to process, it should be as per approved WPS. 
SMAW would be acceptable with same consumables 

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CANDtUcF-8SZ%2BFOoa-TAaFqRO67EKXWL0bB-sjAb_SzhAuMRTpQ%40mail.gmail.com.
--
Thanks & Regards,
Lakshman kumar B
Reply all
Reply to author
Forward
0 new messages