Magnetization of A 335 P11/P12 during grinding process

127 views
Skip to first unread message

B Osare

unread,
Apr 7, 2015, 3:14:33 AM4/7/15
to material...@googlegroups.com
Dear Experts,
 
We have observed that piping material  A 335  P11 & P12 of Super heater Header Tee size 12”& 18” (Thickness 45.00 mm & 65.00 mm respectively)  was magnetized during grinding process at Location (not in workshop).   Can anyone tell us how this phenomenon occurs and how it can be de-magnetize at job location? The weld material is getting cracked after welding. Please suggest the  welding procedure with suitable welding electrodes & what precautions  to be taken during welding.
 
 
Regards
 
B Osare
From National Fertilizers Limited, Vijaipur

Don Under Survilliance

unread,
Apr 7, 2015, 6:03:03 AM4/7/15
to material...@googlegroups.com
wrap the copper coils around the job at location and ground it. it will surely help
 

--
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To post to this group, send email to material...@googlegroups.com.
Visit this group at http://groups.google.com/group/materials-welding.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CE2FEBA545354C0C93B2B0585FD87FE4%40mechworkshop.
For more options, visit https://groups.google.com/d/optout.

Manoj Singh

unread,
Apr 7, 2015, 11:40:37 PM4/7/15
to material...@googlegroups.com
Do preheat before welding do demagnetize it

B Osare

unread,
Apr 8, 2015, 12:11:53 AM4/8/15
to material...@googlegroups.com
We have preheated up 250 deg C but no result...please suggest the Preheat Temp.

Chandra

unread,
Apr 8, 2015, 3:13:56 AM4/8/15
to material...@googlegroups.com
Usually during welding, you use earthing connection. Try to add 2 more earthing connections and weld, sure it will demagnetised during welding.
Usually we follow the same for welding of 9%Ni steeel

Sent from my iPhone

Biplab Pal

unread,
Apr 12, 2015, 11:22:17 PM4/12/15
to materials-welding
Dear Mr. B Osare,

Can you please provide me the value magnetism strength.
The solution depends upon that value.
Use Gauss meter for checking & check the direction of magnetism.



On Tue, Apr 7, 2015 at 12:36 PM, B Osare <bos...@nfl.co.in> wrote:

--
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To post to this group, send email to material...@googlegroups.com.
Visit this group at http://groups.google.com/group/materials-welding.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CE2FEBA545354C0C93B2B0585FD87FE4%40mechworkshop.
For more options, visit https://groups.google.com/d/optout.



--
Thanks & Regards
Biplab Pal
Welding Inspector
E-mail:   bipla...@gmail.com
 
Information in this email and any attachments is confidential and intended solely for the use of the individual(s) to whom it is addressed or otherwise directed. Please note that any views or opinions presented in this email are solely those of the author and do not necessarily represent those of the Company. Finally, the recipient should check this email and any attachments for the presence of viruses. Myself accepts no liability for any damage caused by any virus transmitted by this email.
 

Hareesh K V

unread,
Apr 13, 2015, 10:54:56 PM4/13/15
to materials-welding

Dear sir,

We had the issue of magnetism when we had done some modifications in a P11 pipe during shutdown of plant.

What we done is after fitup, we wrapped the welding cable (to be tried with positive and negative cable and wrapping direction as a trail and error method) and welded.

The principle we followed is right hand thumb rule. That is the magnetization developed by the cable should reduce/neutralize the magnetic effect created in the pipe. No of turns of cable will also a factor to increase or decrease the strength.
After welding of 1 or 2 inch length the magnetization will disappeared.

Best Regards

Hareesh K V