PWHT confirmation

98 views
Skip to first unread message

muthu barathi

unread,
Jul 4, 2016, 1:26:00 AM7/4/16
to material...@googlegroups.com

Hi experts,

Contractors carried out the PWHT and graphs available with correct data's.  Due to urgency the contractor has painted and erected. It is CS material.
Now the owner rejected the reports and asking for PWHT again.

Please send me your best answer  if the PWHT is carried again , whether it will affect the welding and material properties and how to prove that PWHT  has been carried out.  How many times the PWHT could be carried out repeatedly.

Please send your replies.

Thanking you.

With Regards,

Muthu Barathi P.


Sent from RediffmailNG on Android

Jignesh Desai

unread,
Jul 4, 2016, 2:00:24 AM7/4/16
to Materials & Welding, muthu_...@rediffmail.com

Yes it is true that by physical appearance (Next day after PWHT), one can say that PWHT is done for CS welds. However, effectiveness of PWHT can also be verified by production hardness test…Let client witness hardness test.

 

If you want to do PWHT more than one time for reason of weld repair or any other, base materials & welding consumables shall be simulated for the more than one time heat treatment to ensure it retaining mechanical properties after required cycle of PWHT.

 

Sometimes job PQR also reflects additional PWHT once, twice, thrice..... as required. Generally it is shown in PQR with extra holding time.


Regds/Jignesh

anand gupta

unread,
Jul 4, 2016, 2:19:51 AM7/4/16
to material...@googlegroups.com
You can prove with hardness test .

PWHT is doing for reduce hardness and relies residual stress.
if hardness value is below the max limit that means pwht done.

Regards
a p gupta



On Mon, 4 Jul, 2016 at 7:30, muthu barathi
--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To post to this group, send email to material...@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/20160704020031.5281.qmail%40f5mail-224-164.rediffmail.com.
For more options, visit https://groups.google.com/d/optout.

Jignesh Desai

unread,
Jul 4, 2016, 2:34:37 AM7/4/16
to Materials & Welding, muthu_...@rediffmail.com

You may also show the internal visual surface of weld joint if accessible. (Either by naked eye or boroscope).


On Monday, 4 July 2016 10:56:00 UTC+5:30, muthu barathi wrote:

Ali Bhatti

unread,
Jul 4, 2016, 8:33:11 PM7/4/16
to material...@googlegroups.com
Check hardness test and crack through PAUT

Sent from my iPhone
--

Jian Xu

unread,
Jul 14, 2016, 11:09:37 PM7/14/16
to Materials & Welding, muthu_...@rediffmail.com
before you do second PWHT, PQR is essential to demonstrate this action is OK.

but  I don't think hardness value can be used to tell PWHT have been done or not.

and pls. note, each PWHT will cause other potential risk, such as, distortion, cracks, scale, out of roundness, excessive oxidation, etc.

 