Matching base metal ABS EH36 and electrode,,,

183 views
Skip to first unread message

chandra putra

unread,
Jan 12, 2013, 12:03:01 AM1/12/13
to materials-welding
dear expert,

i'm have material ABS EH36 (Tensile Range 71-90 Ksi),include on the group II in AWS D1.1
can i used electrode E7016?
how the tensile strength wire electode can be matching with the base metal.
the welding process will be used SMAW.

note:
1.base metal in the WPS include group II but not ABS EH36
2. Electrode used in WPS E7016

Thanks you for you kind attention.
 
Regards,
Chandra Putra
Skype: chandra.putra12

Dick Overkleeft

unread,
Jan 12, 2013, 1:11:50 PM1/12/13
to material...@googlegroups.com
Dear Chandra you can use E7016. You have to take care for the requirement on impact value at -40 degrees C, if applicable.

best regards, Dick

2013/1/12 chandra putra <bocan...@yahoo.com>

--
To post to this group, send email to material...@googlegroups.com
To unsubscribe from this group, send email to materials-weld...@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
 
 

Reply all
Reply to author
Forward
0 new messages