Dear experts,
      Please kindly clarify if we can use ER309L filler wire for dissimilar welding between P1(A106 Gr B) to P8 (A182 F316L) in gas service
 Your valuable suggestion is highly appreciated.

pradip kumar Sil

unread,
Feb 19, 2022, 9:51:52 AM2/19/22
to materials-welding
you can use it if the service temp is not greater than 300-degree centigrade

On Sat, Feb 19, 2022 at 7:51 PM pradip kumar Sil <prad...@gmail.com> wrote:
Yes, you can

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CACZrEUZKfqUesgcm5Z-z8ig%3Dr6KHRedXZk4%2Bg5X9v98vqxf7ZA%40mail.gmail.com.

fikril shaharudin

unread,
Feb 22, 2022, 10:59:21 PM2/22/22
to material...@googlegroups.com
what should we use if the service temperature greater than 300 degree C?


pradip kumar Sil

unread,
Feb 23, 2022, 12:07:59 AM2/23/22
to materials-welding

james gerald

unread,
Feb 23, 2022, 12:08:06 AM2/23/22
to material...@googlegroups.com
From API 582 below.

Inline image


Inline image


Thanks & Regards

J.Gerald Jayakumar




George Dilintas

unread,
Feb 23, 2022, 11:06:47 PM2/23/22
to material...@googlegroups.com

Kannayeram Gnanapandithan

unread,
Feb 28, 2022, 3:33:36 AM2/28/22
to materials-welding
if i use 309, what is the consequences on metallurgical properties.

THANKS & BEST REGARDS,
KG.PANDITHAN, BE, IWE,  CSWIP 3.1,
ISO 9712 Level 2 in VT,
ASNT-Level II in PT,MT,RT & UT,
LA ISO 9001-2015,
International Welding Engineer. 
CONSULTANT-WELDING & QUALITY
Mobile no: +919940739349