regareding taper burning of electrode

88 views
Skip to first unread message

akshay

unread,
Sep 26, 2017, 1:10:13 AM9/26/17
to Materials & Welding
when we starts welding the electrodes starts burning in taper shape please suggest improvement and reason behind it how i can overcome this problem 

Perumal Govindan

unread,
Sep 26, 2017, 2:03:00 AM9/26/17
to material...@googlegroups.com

Hi

I believe it's due to non concentric flux coating of electrodes. It's a manufacturing defect.

Take few electrodes from the pocket inspect visually and measure it's flux coating thickness through vernier caliper and you will find uninformed coating.

Regards
P Govindan

On Sep 26, 2017 08:10, "akshay" <akshaykul...@gmail.com> wrote:
when we starts welding the electrodes starts burning in taper shape please suggest improvement and reason behind it how i can overcome this problem 

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.

PREM SHANKARDUTT NAUTIYAL

unread,
Sep 27, 2017, 10:17:26 PM9/27/17
to material...@googlegroups.com
Its manufacturing defect of consumable manufacturer.

Please tell your consumable manufacturer to replace the defective batch.

PREM S NAUTIYAL
CELL : 9769316004
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.

Suchin K.

unread,
Oct 1, 2017, 4:39:37 AM10/1/17
to material...@googlegroups.com, cen...@skndt.com

Dear Friend and Expert

 

Regarding to Radiographic Testing (RT) of weld

 

1)     Does any codes / stands mentioned how to selection of film type/class like carbon steel and stainless steel?

2)     On the heavy wall thickness plat 70 mm (Sphere Tank) welded by SMAW testing by PAUT were found a lot of defects but re-test by RT Ir-192 doesn’t found any things, Any opinions to recommend

 

 

Thanks and Best Regards

 

 

 

Suchin Katavut

 

 

From: prem_n...@rediffmail.com [mailto:prem_n...@rediffmail.com]
Sent: Thursday, September 28, 2017 12:44 AM
To: material...@googlegroups.com
Subject: Re: [MW:26838] regareding taper burning of electrode

 

Its manufacturing defect of consumable manufacturer.

Please tell your consumable manufacturer to replace the defective batch.

PREM S NAUTIYAL
CELL : 9769316004


From: Perumal Govindan <perumal...@gmail.com>
Sent: Tue, 26 Sep 2017 11:32:54
To: material...@googlegroups.com
Subject: Re: [MW:26836] regareding taper burning of electrode
 

Hi

I believe it's due to non concentric flux coating of electrodes. It's a manufacturing defect.

Take few electrodes from the pocket inspect visually and measure it's flux coating thickness through vernier caliper and you will find uninformed coating.

Regards
P Govindan

On Sep 26, 2017 08:10, "akshay" <akshaykul...@gmail.com> wrote:

when we starts welding the electrodes starts burning in taper shape please suggest improvement and reason behind it how i can overcome this problem 

 

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.

To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.

Reply all
Reply to author
Forward
0 new messages