Branch connections & RF pad

118 views
Skip to first unread message

ABHISHEK GHOSH

unread,
Sep 5, 2012, 4:54:57 PM9/5/12
to material...@googlegroups.com
Dear Experts .. 

Please clarify :: 

Q1. In Branch connection , Usage of RF pad depends upon which factors??. Is B 31.3 states any requirement ?? 

Q2. Which code specifies dimension  of "Bar Tee" used for pipeline Pigging? ( 52 " ) ? 

Q3. In our project , we have to weld 52 " ( 19.1 mm)  x 18 "( std sch)  branch ( Stub In)  with RF pad. Header pipe thickness 19.1 mm.In ISO, it is mentioned to use RF pad of thickness 38.2 mm, But we have material of 19.1 mm thickness at site , issued by client.

 Is it really possible to weld two 19.1 mm ( 2 x 19.1 mm= 38.2  mm) Rf pad  to make it 38.2mm ?? If yes , what will be the weld joint configuration??

Thank you for your valuable time. 

With Regards. 
 

ABHISHEK GHOSH 

 


Raghuram Bathula

unread,
Sep 6, 2012, 7:06:48 AM9/6/12
to material...@googlegroups.com
Please use separate thread for these questions (Q2 is not relevant to the subject)

A1. Added reinforcement is required when calculated as per para 304.3.3.b. Thickness selected will depend on the area of reinforcement. check with your designer.

A2. Bar Tees are utilized in a pig launcher/receiver system and/or at branches in the pipeline to ensure the safe passage of a pig past the open branch area. Manufactured as a special item.

Ammar Shaikh

unread,
Sep 7, 2012, 12:39:27 AM9/7/12
to material...@googlegroups.com
Verify the thickness required from formula stated in ASME B 31.3 para 304.3.3.b.
Designers usually keep thickness of RF pad on higher side because welding of thinner RF pads can cause twisting. If this is the case weld it in 4 peices.
If you want to weld two peices and achieve combined thickness then try the following procedure
Weld one pad. Place the other one over it. Drill holes of 12 - 16 mm on the second pad and fill them by welding fusing them with bottom pad. Tack weld at several places.
 
Ammar Shaikh

On Thu, Sep 6, 2012 at 4:46 PM, Alpesh Sakhreliya <alpeshsa...@gmail.com> wrote:
2)  MSS SP 75 & ASME 16.49  FOR USE "BAR TEE" AND FLOW TEE


ALPESH SAKHRELIYA
--
To post to this group, send email to material...@googlegroups.com
To unsubscribe from this group, send email to materials-weld...@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 