Duplex WPS for Super Duplex

158 views
Skip to first unread message

Alex Kumar Antony

unread,
Dec 15, 2025, 8:29:07 AM12/15/25
to Materials & Welding
Can we use Duplex WPS for Super Duplex, kindly quote with the help of code
Thanks

Karunakaran Karan

unread,
Dec 15, 2025, 8:37:03 AM12/15/25
to material...@googlegroups.com
Sir,
 Not using .because filler,interpass temp.,etc are not same.DSS. 
DSS. ER2209 
SDSS ER2594

   Thanks and regards,

     S.KARUNAKARAN,
      karu...@gmail.com
      91-6382279754
      




On Mon, 15 Dec 2025, 16:29 Alex Kumar Antony, <alexk...@gmail.com> wrote:
Can we use Duplex WPS for Super Duplex, kindly quote with the help of code
Thanks

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To view this discussion visit https://groups.google.com/d/msgid/materials-welding/ee5dcbf4-b6cb-4421-8338-04e109d45b15n%40googlegroups.com.

Anandhapadmanabha pillaim

unread,
Dec 15, 2025, 11:35:42 AM12/15/25
to material...@googlegroups.com
As per ASME Section IX, the use of SDSS filler wire is permitted even when impact testing is not specified or required, provided the essential variables are met.

However, beyond the code requirements, from a metallurgical and performance standpoint, DSS and SDSS differ significantly in their ferrite-austenite phase balance requirements. Achieving the correct phase balance is critical and is strongly influenced by welding heat input. SDSS, in particular, has a higher PREN (Pitting Resistance Equivalent Number) requirement compared to DSS.

To achieve the required PREN and phase balance in SDSS weld metal, nitrogen is commonly added to the shielding and backing gas. Nitrogen is a strong austenite stabilizer and also contributes to an increase in PREN, thereby improving corrosion resistance.

If a WPS is qualified for DSS using pure argon as the shielding gas, and it is later proposed to use an argon–nitrogen mixture (for Eg: Ar + 2% N₂) for SDSS welding, this change would require requalification of the PQR. This is because the addition of nitrogen significantly affects weld metal chemistry, phase balance, and mechanical and corrosion properties, making it a metallurgically significant change even if not explicitly listed as an essential variable in all cases.

That said, if the required mechanical properties, corrosion resistance, and phase balance are successfully achieved using the same gas composition qualified for DSS (i.e., pure argon), ASME Section IX permits its use, as long as all applicable essential and supplementary essential variables remain within the qualified range.

On Mon, 15 Dec 2025, 5:29 pm Alex Kumar Antony, <alexk...@gmail.com> wrote:
Can we use Duplex WPS for Super Duplex, kindly quote with the help of code
Thanks

--

syed kauser ahmed

unread,
Dec 15, 2025, 11:35:44 AM12/15/25
to material...@googlegroups.com
As per ASME Section IX – QW-403.5:

No, a change from one Group Number to another Group Number within the same P-Number shall be considered an essential variable and requires requalification of the WPS.

On Mon, 15 Dec 2025, 16:29 Alex Kumar Antony, <alexk...@gmail.com> wrote:
Can we use Duplex WPS for Super Duplex, kindly quote with the help of code
Thanks

--

Mohd Siraj

unread,
Dec 15, 2025, 11:35:45 AM12/15/25
to Materials & Welding
yes, provided that you have revised drawing.

venkateswara reddy Desireddy

unread,
Dec 15, 2025, 10:12:59 PM12/15/25
to material...@googlegroups.com
Yes you are right, shielding gas also one of the essential variables. Along with P number and F number other parameters also we have to consider before choosing WPS.


Marco Nunes

unread,
Dec 15, 2025, 10:13:00 PM12/15/25
to material...@googlegroups.com

Code-Based Explanation (ASME Section IX)

1. Base Material Grouping – P-Numbers

ASME Section IX groups materials by P-Numbers to control essential variables.

  • Duplex Stainless Steels (e.g., UNS S31803 / S32205)
    P-No. 10H

  • Super Duplex Stainless Steels (e.g., UNS S32750 / S32760)
    P-No. 10I

📌 Since P-No. 10H ≠ P-No. 10I, they are treated as different base material groups.


2. Essential Variable for Base Materials

ASME Section IX clearly states:

QW-403.11
A change from one P-Number to another P-Number is an essential variable and requires requalification of the WPS.

✅ Therefore:

  • A WPS qualified on Duplex (P-No. 10H)

  • Cannot be used for Super Duplex (P-No. 10I)

  • Without a new PQR covering P-No. 10I


3. Mechanical and Metallurgical Differences (Supporting Rationale)

Although not strictly required by code, this reinforces why the rule exists:

  • Super Duplex has:

    • Higher PREN

    • Higher yield and tensile strength

    • Tighter control on heat input, interpass temperature, and ferrite/austenite balance

  • Welding Super Duplex with a Duplex-qualified WPS risks:

    • Loss of corrosion resistance

    • Sigma phase formation

    • Improper phase balance

Codes intentionally separate these alloys due to these risks.


4. Filler Metal Consideration (Additional Control)

Even if a Super Duplex filler metal is used, the limitation still applies, because:

QW-404 (Filler Metal Essential Variables)
Filler metal control does not override base material P-Number limitations.


Final Conclusion (Code-Compliant Answer)

A Duplex WPS cannot be used for Super Duplex welding.

ASME Section IX requires requalification, because:

  • Duplex = P-No. 10H

  • Super Duplex = P-No. 10I

  • Change in P-Number is an essential variable per QW-403.11


On Mon, Dec 15, 2025 at 9:28 AM Alex Kumar Antony <alexk...@gmail.com> wrote:
Can we use Duplex WPS for Super Duplex, kindly quote with the help of code
Thanks

--

Anandhapadmanabha pillaim

unread,
Dec 15, 2025, 10:13:06 PM12/15/25
to material...@googlegroups.com
Base material grouping is a supplymentary essential variable, even though it's a supplymentary essential variable, both DSS & SDSS have P 10H and Gr. 1. As per ASME SDSD WPS is permitted to write with DSS PQR, still impact testing is not there you want to use SDSS wire itself, yes it is permitted, if impact testing is there and you want to use SDSS wire, it's not permitted and requalification is required, 

Below consideration I have addressed previous need to be taken into consideration, 

However, beyond the code requirements, from a metallurgical and performance standpoint, DSS and SDSS differ significantly in their ferrite-austenite phase balance requirements. Achieving the correct phase balance is critical and is strongly influenced by welding heat input. SDSS, in particular, has a higher PREN (Pitting Resistance Equivalent Number) requirement compared to DSS.

To achieve the required PREN and phase balance in SDSS weld metal, nitrogen is commonly added to the shielding and backing gas. Nitrogen is a strong austenite stabilizer and also contributes to an increase in PREN, thereby improving corrosion resistance.

If a WPS is qualified for DSS using pure argon as the shielding gas, and it is later proposed to use an argon–nitrogen mixture (for Eg: Ar + 2% N₂) for SDSS welding, this change would require requalification of the PQR. This is because the addition of nitrogen significantly affects weld metal chemistry, phase balance, and mechanical and corrosion properties, making it a metallurgically significant change even if not explicitly listed as an essential variable in all cases.

That said, if the required mechanical properties, corrosion resistance, and phase balance are successfully achieved using the same gas composition qualified for DSS (i.e., pure argon), ASME Section IX permits its use, as long as all applicable essential and supplementary essential variables remain within the qualified range.

Anandhapadmanabha pillaim

unread,
Dec 15, 2025, 11:29:02 PM12/15/25
to material...@googlegroups.com
Please don't share wrong information both are P 10H Gr. 1 only refer QW/QB- 422


Mohmmed Dudhiyawala

unread,
Feb 2, 2026, 5:49:46 AMFeb 2
to Materials & Welding
DSS and SDSS are same group no. as per ASME IX. i.e. P10H G1

james gerald

unread,
Feb 2, 2026, 7:03:26 AMFeb 2
to material...@googlegroups.com
Super Duplex have a Tensile strength of 115ksi whereas duplex have a Tensile strength of 95 ksi.

You cannot use a duplex PQR to weld super duplex SS though P.No/F.No/A.No(if used super duplex) are same but additional requirements like Corrosion test restricts them

Thanks & Regards

J.Gerald Jayakumar

0091-8838619635