Sulfuric acid drum nozzle problem

39 views
Skip to first unread message

okay Tutar

unread,
Mar 30, 2021, 4:31:05 AM3/30/21
to Materials & Welding
Hello everyone, I hope you all have a nıce day.

We had a problem in sulfuric acid %99 conct. drum nozzle.

After 2 years of operation, suddenly our nozzle has been failured.
We checked api 571.Concentration of acid is ok, it is %99.Speed of acid is lower than critical level.
But, when we examine flange and piping of nozzle. There is general corrosion and thickness of weld neck is thinned . Our material is carbon steel. But, in pipe thickness is not thinned.
Do you have suggestion for reason of this problem ? What could it be ?

Vinoth kanna ramachandran

unread,
Mar 30, 2021, 7:02:08 AM3/30/21
to material...@googlegroups.com
Dear sir,

Greetings 

kindly  make sure that the pipe thickness is not thinned using DIGITAL RT if possible.  

We experienced the same problem in repair of sulphuric acid vertical mounted vessel , Carbon steel A 516  Gr B , nozzle failure . 

later we found under deposit corrosion of nozzle pipes . the we back gouged and flush grounded with E-316 for repair. 

please update , if you got better solution. 



Regards

Vinoth kanna
QC- welding & piping inspector 
Manifa Project

API -510, CSWIP 3.1, NDT level II - UT, RT ,PT, MT, VT,LT,Infrared & Thermography 
Technical - Metallurgy

Contact : M - +91-9787954338,+966-539127946
              Email id : srvk...@gmail.com


--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/d4b67686-33e7-429b-9ebc-9e16768ddb8cn%40googlegroups.com.

chandrakant mohikar

unread,
Mar 30, 2021, 11:14:02 PM3/30/21
to material...@googlegroups.com
Nozzle failed means, what exactly happened.?  if no flow through nozzle means, it is choked. it should be dechoked and material like dirt etc to be removed, another reason may be there is some other corrosive material through reverse flow. you can conduct systematically risk / HAZOP study with guidewords. if you can isolate, drain 99% H2SO4, remove nozzle and perfoem QA / TIC (testing, inspection & certification). as per design & EPC requirements, considerations & criteria. 

chandrakant mohikar


  

--

Zohair.O

unread,
Apr 1, 2021, 2:51:58 AM4/1/21
to Materials & Welding
Hi everyone, 

Sulfuric acid is very tricky when we talk about corrosivity because it depends on many factors ( concentration, temperature, velocity ... etc). For the concentration of 98% generally, it's better to use the SS316 instead of carbon steel for pipes, and you may use the carbon steel tanks with SS clad or overlaid nozzles. 
I thank the problem is mainly related to material selection.    
you can consult the NACE Standard related to sulfuric acid storage tank inspection. 

Z.O

okay Tutar

unread,
Apr 30, 2021, 8:48:36 AM4/30/21
to Materials & Welding
Dear zohair,

Thank you for your help! We have decided to use SS316 steel instead of carbon steel. Problem is actually because of sulphuric acid corrosion.

Kind regards,