purpose of doing nick-break test.

634 views
Skip to first unread message

bas karan

unread,
Oct 30, 2010, 5:53:23 AM10/30/10
to material...@googlegroups.com
Dear all
pls explain if any one know the purpose of doing nick-break test.

Thanks&regards
Baskaran.


saRAVANAN

unread,
Oct 31, 2010, 3:56:58 AM10/31/10
to material...@googlegroups.com
Dear Mr Baskaran,

This test is performed to reveal internal imperfections such as slag inclusion, lack of fusion, incomplete penetration, porosity, etc in a butt weld.  A butt weld specimen is fractured along an artificial notch that is intentionally machined on the centre line of the fillet weld specimen to facilitate fracture in the centre of the weld. The fractured specimen cross section is then visually examined for imperfections.




--
To post to this group, send email to material...@googlegroups.com
To unsubscribe from this group, send email to materials-weld...@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

Shashank Vagal

unread,
Oct 31, 2010, 9:35:40 AM10/31/10
to material...@googlegroups.com
Other intention is to get a measure of the ductility of the joint at the bend location.

--- On Sun, 31/10/10, saRAVANAN <vivid...@gmail.com> wrote:

waqqaar waqqaar

unread,
Oct 31, 2010, 10:24:38 AM10/31/10
to material...@googlegroups.com
The NICK-BREAK TEST is useful for determining the internal quality of the weld metal. This test reveals various internal defects (if present), such as slag
inclusions,  gas  pockets,  lack  of  fusion,  and  oxidized  or burned metal. To accomplish the nick-break test for checking a butt weld, you must first flame-cut the test specimens from a sample weld . Make a saw cut at each edge through the center of the weld

 thanx

Hafiz Waqar Zia 
Etimaad Qatar LL.C
QA/QC Dept.
Doha  Qatar
Cell: +97466598936
Email- Waqq...@hotmail.com 

 





 

Date: Sun, 31 Oct 2010 11:56:58 +0400
Subject: Re: [MW:7961] purpose of doing nick-break test.
From: vivid...@gmail.com
To: material...@googlegroups.com

bas karan

unread,
Nov 1, 2010, 6:04:00 AM11/1/10
to material...@googlegroups.com
 Dear sir
 
all the inperfection u mentioned can be detected by RT.then why we are doing nick-break.
 
pls explain in engineering point of view not inspection.
thank you.
Regards
Baskaran.




--- On Sun, 31/10/10, Shashank Vagal <nach...@yahoo.com> wrote:

hpi001

unread,
Nov 1, 2010, 11:02:29 AM11/1/10
to Materials & Welding
The Nick break test will also show any present lack of fusion between
the separate weld layers or on the weld bevels. During RT you won't
find such because of the radiation direction.

Best Regards,

Herman Pieper

narasimha murthy

unread,
Nov 1, 2010, 11:59:17 AM11/1/10
to material...@googlegroups.com
 
The purpose of Nick Break Test - A nick break test involves breaking the weld joint to examine the fractured surfaces for internal defects such as:
(i) Gas pockets
(ii) Slag inclusions
(iii) Porosity.
The test also determines weld ductility and the degree of fusion.

Regards
 
J.N.Murthy