WPS as per ASME SEc. IX

106 views
Skip to first unread message

Manoj John

unread,
Nov 18, 2016, 9:59:26 PM11/18/16
to material...@googlegroups.com
Dear Experts,

We have the following WPS as per ASME Sec. IX

Base metal - P5B + P8  (6" Sch 40 Pipe)
Welding process -  GTAW
Filler metal -  ER NiCr-3
Preheat temp - 180 degree C
PWHT - Nil
Trailing & backing gas -  Yes (Argon)

Can i use the above procedure for welding of ;

P5B group material fillet welding (seal welding of threaded joints) with ER NiCr-3 or ER NICrMo-3 GTAW process without PWHT 
Hardness test required for HAZ 235HV10.

your expert advice highly appreciated.

Thanks & Regards,
Manoj.

Kurniatullah Sirajudin

unread,
Nov 19, 2016, 1:12:37 AM11/19/16
to Materials & Welding
if this WPS will be applied for oil and gas service, you can refer to API RP 582 table A, and ASME IIC for selection wleding consumable

Regards
Kurniatullah Sirajudin

George Dilintas

unread,
Nov 20, 2016, 9:24:06 PM11/20/16
to Meghanadh K
let us take the some essential variables one by one:
Pno: see QW 403.11 and then QW 424. The combination you have does not help. It qualifies only PNo 5B to Pno *.
A no: due to the dilution between a low alloy and stainless steel most probably it will not match.

So no chance, you need a new PQR

--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CACgUO5nE%3DtZ-gmMz2cg%3DzBTMjGpOTCxSxUQwT7jSRDWn3SkFXw%40mail.gmail.com.
For more options, visit https://groups.google.com/d/optout.



--
Dr. Georgios Dilintas,
Dipl. Ing. In Aeronautic and Space Engineering
Ph.D in Mechanics of Solids - Computational Mechanics
A.I.S, A.N.I, IRCA Lead Auditor
Welding, Stress Analysis, Corrosion, QA/QC, Failure Analysis, Risk Analysis