Regarding PWHT as per B31.3 and B31.1

135 views
Skip to first unread message

K K

unread,
Jul 13, 2019, 11:16:14 AM7/13/19
to Materials & Welding
Dear All,

I have query about PWHT,

I have qualified WPS and PQR, as per B31.3.(But our requirements as per B31.3 and B31.1 )

Can you please tell me some one, what is difference between theses both standard for PWHT.  

( As per my knowledge  1) PWHT temperature for ASME P number 04 material is different from ASME B31.3 (process) : range 704-746°C to ASME B31.1 (Power) : range 650-700°C.)

Below I have given some WPS parameters for PWHT, please clarify me whether the parameters are correct or Not. 

According to B31.3 -

Material : ASTM A 335 P11 to ASTM A 335 P11 - ( PNo-4; G.No-1 to PNo-4; G.No-1 )
Process : GTAW
Test coupon Thickness :  19.05 mm
PWHT- Temp range - 690°C- 705°C
Heating range : 200°C/hr
Cooling range : 200°C/hr
Interpass temp : 315°C
Post Heating : 300°C -350°C ; holding thickness 10mm to 20mm -30 min / 20mm to 30mm - 90min.

And regarding Backing -  PQR is qualified with Argon, can we use Nitrogen in WPS.

Experts i am looking your favorable reply on my query.

Thanks

Kiran

munee...@gmail.com

unread,
Jul 15, 2019, 1:34:53 AM7/15/19
to materials-welding
Greetings,

I hope youre into power generations, where you touch, boilers, power and process...

Find my reply below in green, rest acceptable..

( As per my knowledge  1) PWHT temperature for ASME P number 04 material is different from ASME B31.3 (process) : range 704-746°C to ASME B31.1 (Power) : range 650-700°C.)

Reply:  I have 2016, 31.3 vs 12, 31.1, which does not has this major difference for P no 4,  to be precise (.3) comes with 650 to 705, where as (.1) with 650 to 700, which is acceptable. there are other P nos which has more than 5 Deg variations, which is not your case.

Below I have given some WPS parameters for PWHT, please clarify me whether the parameters are correct or Not. 

According to B31.3 -

Material : ASTM A 335 P11 to ASTM A 335 P11 - ( PNo-4; G.No-1 to PNo-4; G.No-1 )
Process : GTAW
Test coupon Thickness :  19.05 mm

Reply: why do you go with full GTAW for 19.05??

PWHT- Temp range - 690°C- 705°C

Reply: 690 is ok

Heating range : 200°C/hr
Cooling range : 200°C/hr
Interpass temp : 315°C  
Post Heating : 300°C -350°C ; holding thickness 10mm to 20mm -30 min / 20mm to 30mm - 90min.

Reply: i made something like this and approved, A minimum of 25% of the groove weld is filled, the weldment is sufficiently supported with Post heating gradually increasing as per the WPS requirement 400 deg C  at 2 hours after the welding completion, the bottom line is started after 25% with gradual fullfilled post heating after weld completion for continous 2 hours at 400 deg C.

And regarding Backing -  PQR is qualified with Argon, can we use Nitrogen in WPS.

Reply: read QW-408.2.


Yours
MOHAMED MUNEEB MAHABOOB
+91-786-700-444-6      TRZ - INDIA

''The first man landed on earth has reference still today - so anything you do in your life check for reference, if you dont find then what you are doing is wrong, try to find''

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/270bf5d4-65f6-4e9c-bea5-331611e4edfe%40googlegroups.com.